Study of Polyaniline/Silicon Dioxide based Coating on Carbon Steel in Artificial Geothermal Brine
- By using the available resources in Indonesia, such as silicon dioxide and marine coating base, the PANI/SiO2 modified alkyd coating was able to protect carbon steel in a deaerated artificial geothermal water. The screening of coatings shows that the modification by adding individual pigment was not sufficient to protect carbon steel even during a short-term exposure, indicated by the discoloration after only seven days of exposure. Electrochemical tests indicated that there was no significant change in the Ecorr between the coated and uncoated carbon steel at room temperature. At 150 °C, the coated carbon steel has a lower potential than that of carbon steel, indicating that the coating is protecting carbon steel cathodically or slowing down the corrosion reaction. Finally, a long-term exposure test confirmed that the PANI/SiO2 modified coating successfully protects the carbon steel in the Sibayak artificial geothermal water up to 150 °C for 6 months.