Ingenieurwissenschaften und zugeordnete Tätigkeiten
Filtern
Dokumenttyp
- Sonstiges (35)
- Vortrag (24)
- Beitrag zu einem Tagungsband (22)
- Zeitschriftenartikel (10)
- Forschungsbericht (2)
Referierte Publikation
- nein (93) (entfernen)
Schlagworte
- Corrosion (45)
- Geothermal (17)
- Korrosion (13)
- Coating (10)
- CCS (9)
- Steel (9)
- Copper (7)
- Polyaniline (7)
- CCUS (6)
- CCU (5)
Organisationseinheit der BAM
- 7 Bauwerkssicherheit (93) (entfernen)
Eingeladener Vortrag
- nein (24)
Since 2016 ISO Technical Committee (TC) 265 is working on standardization the whole CCS-process chain. Around 30 countries are working together to provide international guidelines. As ISO 27913 was the first standard finished within these activities it is already in the stage of first revision.
The objective of ISO 27913 is “to provide specific requirements and recommendations on certain aspects of safe and reliable design, construction and operation of pipelines intended for the large-scale transportation of CO2 that are not already covered in existing pipeline standards such as ISO 13623, ASME B31.8, EN 1594, AS 2885 or other standards. Existing pipeline standards cover many of the issues related to the design and construction of CO2 pipelines; however, there are some CO2 specific issues that are not adequately covered in these standards. The purpose of this document is to cover these issues consistently. Hence, this document is not a standalone standard, but is written to be a supplement to other existing pipeline standards for natural gas or liquids for both onshore and offshore pipelines.”
This contribution shall provide information on the content, the current stage of the revision process, encourage to contribute to this standard and make listeners aware to consider the influence of ISO standard on documents currently in draft.
Since 2016 ISO Technical Committee (TC) 265 is working on standardization the whole CCS-process chain. Around 30 countries are working together to provide international guidelines. As ISO 27913 was the first standard finished within these activities it is already in the stage of first revision.
The objective of ISO 27913 is “to provide specific requirements and recommendations on certain aspects of safe and reliable design, construction and operation of pipelines intended for the large-scale transportation of CO2 that are not already covered in existing pipeline standards such as ISO 13623, ASME B31.8, EN 1594, AS 2885 or other standards. Existing pipeline standards cover many of the issues related to the design and construction of CO2 pipelines; however, there are some CO2 specific issues that are not adequately covered in these standards. The purpose of this document is to cover these issues consistently. Hence, this document is not a standalone standard, but is written to be a supplement to other existing pipeline standards for natural gas or liquids for both onshore and offshore pipelines.”
This contribution shall provide information on the content, the current stage of the revision process, encourage to contribute to this standard and make listeners aware to consider the influence of ISO standard on documents currently in draft.
Durch Auslagerungs- und elektrochemische Tests im Labor kann das Korrosionsverhalten verschiedener metallener Werkstoffe beurteilt werden. Aus den Versuchsergebnissen, die in verschiedenen synthetischen Geothermalwässern im Labor erzielt wurden, lassen sich die folgenden Schlussfolgerungen ziehen:
• Die Anfälligkeit für Spaltkorrosion wurde als wichtigster Aspekt für die Werkstoffqualifizierung ermittelt.
• Der niedriglegierte Stahl 25CrMo4 zeigte bei niedrigem Salzgehalt in MB-Geothermalwasser eine gleichmäßige Korrosion unterhalb der akzeptierten Schwelle von 0,3 mm/Jahr. Daher kann er als geeignet für geothermische Bedingungen mit niedrigem Salzgehalt angesehen werden, wie sie für MB getestet wurden. Es besteht keine Notwendigkeit, auf höherlegierte (teurere) Werkstoffe auszuweichen. Ein niedrigerer pH-Wert (wie bei LHD) führt zu Korrosionsraten oberhalb der akzeptablen Grenzwerte, so dass die niedriglegierten Werkstoffe nicht für Flüssigkeiten mit niedrigem pH-Wert geeignet sind.
• Stark salzhaltige Geothermalwässer erfordern höherlegierte Werkstoffe, da die Korrosionsrate von niedriglegiertem Stahl zu hoch ist.
• Der Duplexstahl X2CrNiMo22-5-3 und der Superduplexstahl X2CrNiMoCuWN25-7-4 wurden aufgrund ihrer kritischen Anfälligkeit für örtliche Korrosion in Form von Loch- und Spaltkorrosion unter Betriebsbedingungen nicht als geeignet für geothermische Anwendungen in Geothermalwässern mit einer mit NDB und ORG vergleichbaren Zusammensetzung angesehen.
• Der superaustenitische Stahl X1CrNiMoCu32-28-7 eignet sich für ORG und salzarme Wässer. In NDB-Geothermalwasser wurde er bei 100 °C als geeignet angesehen. Jedoch schränkt seine Anfälligkeit für Spaltkorrosion seine Anwendbarkeit ein. Neben seiner guten Korrosionsbeständigkeit ist sein Repassivierungsverhalten für seine begrenzte Anwendbarkeit in Geothermalwässern mit niedrigem pH-Wert verantwortlich.
• Die Nickelbasislegierung NiCr23Mo16Al wurde als geeignet erachtet und stellt eine sichere Option für den Einsatz in geothermischen Anlagen dar, selbst wenn mit stark salzhaltigem Geothermalwasser gearbeitet wird.
Durch Auslagerungs- und elektrochemische Tests im Labor kann das Korrosionsverhalten verschiedener metallener Werkstoffe beurteilt werden. Aus den Versuchsergebnissen, die in verschiedenen synthetischen Geothermalwässern im Labor erzielt wurden, lassen sich die folgenden Schlussfolgerungen ziehen:
• Die Anfälligkeit für Spaltkorrosion wurde als wichtigster Aspekt für die Werkstoffqualifizierung ermittelt.
• Der niedriglegierte Stahl 25CrMo4 zeigte bei niedrigem Salzgehalt in MB-Geothermalwasser eine gleichmäßige Korrosion unterhalb der akzeptierten Schwelle von 0,3 mm/Jahr. Daher kann er als geeignet für geothermische Bedingungen mit niedrigem Salzgehalt angesehen werden, wie sie für MB getestet wurden. Es besteht keine Notwendigkeit, auf höherlegierte (teurere) Werkstoffe auszuweichen. Ein niedrigerer pH-Wert (wie bei LHD) führt zu Korrosionsraten oberhalb der akzeptablen Grenzwerte, so dass die niedriglegierten Werkstoffe nicht für Flüssigkeiten mit niedrigem pH-Wert geeignet sind.
• Stark salzhaltige Geothermalwässer erfordern höherlegierte Werkstoffe, da die Korrosionsrate von niedriglegiertem Stahl zu hoch ist.
• Der Duplexstahl X2CrNiMo22-5-3 und der Superduplexstahl X2CrNiMoCuWN25-7-4 wurden aufgrund ihrer kritischen Anfälligkeit für örtliche Korrosion in Form von Loch- und Spaltkorrosion unter Betriebsbedingungen nicht als geeignet für geothermische Anwendungen in Geothermalwässern mit einer mit NDB und ORG vergleichbaren Zusammensetzung angesehen.
• Der superaustenitische Stahl X1CrNiMoCu32-28-7 eignet sich für ORG und salzarme Wässer. In NDB-Geothermalwasser wurde er bei 100 °C als geeignet angesehen. Jedoch schränkt seine Anfälligkeit für Spaltkorrosion seine Anwendbarkeit ein. Neben seiner guten Korrosionsbeständigkeit ist sein Repassivierungsverhalten für seine begrenzte Anwendbarkeit in Geothermalwässern mit niedrigem pH-Wert verantwortlich.
• Die Nickelbasislegierung NiCr23Mo16Al wurde als geeignet erachtet und stellt eine sichere Option für den Einsatz in geothermischen Anlagen dar, selbst wenn mit stark salzhaltigem Geothermalwasser gearbeitet wird.
Since geothermal wells are a feasible energy source to replace fossil fuel supply, many technologies have been developed to take advantage of geothermal energy. Nevertheless, service conditions in geothermal facilities are in many cases extreme in terms of corrosion due to the chemical composition of hydrothermal fluids and temperatures. Therefore, materials selection based on preliminary material qualification is essential to guarantee a secure and reliable operation of the facilities. During operation of a geothermal research facility in Groß Schönebeck copper and lead effects have been found downhole. Occurring mechanisms and measures to prevent precipitation or scaling needed to be investigated as well as potential influences of such precipitates on corrosion resistance of metallic materials used for equipment.
This contribution deals with the evaluation of the corrosion behavior of carbon steel and corrosion resistant alloys in copper and/or lead containing artificial geothermal water, simulating the conditions in the Northern German Basin.
The behavior of these materials in an artificial geothermal water obtained by electrochemical measurements and exposure tests are presented. While carbon steel exhibits precipitation and deposition, higher alloyed material shows different response to such species and a higher resistance in saline geothermal water.
Basing on these results the suitability of the investigated corrosion resistant alloy is given for use in such conditions, whereas carbon steel creates difficulties due to its susceptibility to Cu- and Pb-precipitation.
Significant Cu-deposition and precipitation only occurred in combination with carbon steel. High-alloyed materials prevent the disturbing Cu-agglomeration. Pb-deposition and precipitation only occurred in combination with carbon steel. No negative Pb-effect could be observed in combination with high-alloyed steels. High alloyed corrosion resistant alloys are suitable and shall be chosen for future design of the piping system, either in massive or in cladded form, to prevent unwanted interactions with brine components.
The screening of coatings shows that the modification by adding individual pigment was not sufficient to protect carbon steel even during a short-term exposure, indicated by the discoloration after only seven days of exposure.
Electrochemical tests indicated that the coating cathodically protects carbon steel or slows down the corrosion reaction.
A long-term exposure test confirmed that the PANI/SiO2 modified coating successfully protects the carbon steel in the Sibayak artificial geothermal water at 150 °C for 6 months.
Corrosive geothermal brines are a major challenge to geothermal power-plants. For cost reasons, plant designers favorize low alloyed steels, e.g., carbon steel, which are susceptible to uniform and localized corrosion when exposed to geothermal brines having acidic and saline properties. To solve such problem, coatings or inhibitors would be a protective solution as an alternative to the use of high alloyed materials.
This study investigated a coating system consisting of polyaniline/silicon dioxide basing on locally available resources. Protection against corrosion of carbon steel is shown by long-term exposure and electrochemical tests of coated carbon steels, performed in an artificial acidic and saline geothermal brine, comparable to real conditions at a site in Indonesia.
Therefore, an integrated coating system is presented for corrosion protection, combining the electro-chemical functionality of polyaniline and the physical advantages of silica.
Evaluation of corrosion resistance of metallic materials is essential to assure safe and reliable operation of geothermal sites. One need to be aware that corrosion is not a material's but a system property, determined by medium, material and construction aspects. Various corrosion types have to be evaluated. Conditions in laboratory shall reflect on-site reality. Depending on brine composition and temperature suitability of metallic materials can be ranked. Most important outcome of the research is that highly saline geothermal brines require high alloyed materials, for safe long-term operation.
Integrated Coating System for Corrosion Protection of Carbon Steel in Artificial Geothermal Brine
(2022)
Corrosive geothermal brines are a major challenge to geothermal power-plants. For cost reasons, plant designers prefer to use carbon and low alloyed steels, which are susceptible to uniform and localized corrosion when exposed to geothermal brines having acidic and saline properties. To solve such problem, coatings or inhibitors would be a protective solution as an alternative to the use of high alloyed materials.
This study investigated a coating system consisting of polyaniline/silicon dioxide based on resources locally available in Indonesia. Protection against corrosion of carbon steel was shown by long-term (28 day) exposure and electrochemical tests of coated carbon steels, performed in an artificial acidic and saline geothermal brine, comparable to the conditions encountered at a site in Indonesia.
Therefore, an integrated coating system is proposed for corrosion protection, combining the electrochemical functionality of polyaniline and the physical advantages of silica.
Significant Cu-deposition and ‑precipitation only occurred in combination with carbon steel. High-alloyed materials prevent the disturbing Cu-agglomeration. Pb-deposition and ‑precipitation only occurred in combination with carbon steel. No negative Pb-effect could be observed in combination with high-alloyed steels. High alloyed corrosion resistant alloys are suitable and shall be chosen for future design of the piping system, either in massive or in cladded form, if formation of crevices with non-metallic materials can be excluded!
To reveal the corrosion resistance of casing steel/mortar interface in CO2 injection condition, sandwich samples were prepared and exposed up to 20 weeks in aquifer fluid under 10 MPa and 60 °C. Cross section analysis revealed the crevice corrosion as main mechanism instead of pitting corrosion, which would be expected to happen in the extremely high Chloride concentration. Detailed analysis using EDS line scan shown the slow diffusion of Chloride, suggesting why pitting did not happen after 20 weeks. To mimic the passivated steel surface, the steel coupon was passivated in simulated pore solution having pH 13.5 for 42 days. The passivated coupon was further exposed to NGB solution for 28 days. Electrochemical characterization was performed along the exposure processes to reveal the change in impedance, indicating the corrosion resistance of steel casing/mortar interface.
Commercially available carbon steels are suitable for compression and pipelines as long as moisture content and impurities are limited. (water 50 to 100 ppmv, SO2 and NO2 ca. 100 ppmv) Corrosion rates increase with increasing water content. (0.2 – 20 mm/a) Condensation of acids and therefore droplet formation is always possible, even at low water contents. A low SO2 content within the CO2-stream might be more important than a low water content. Cr13-steels showed a general susceptibility to shallow pitting and pitting. So, they seem to be not suitable for CCUS applications. Low alloyed steels showed better corrosion behavior (predictable uniform corrosion). For direct contact with saline aquifer fluids only high alloyed steels shall be used.
The suitability of an Al2O3 coating for corrosion protection on X20Cr13 was evaluated in various artificial geothermal brines, focusing on the influence of different pH (4, 6 and 8) and their chemical compositions on the coating properties. All experiments were performed in the laboratory using autoclaves at 150 ◦C and 1 MPa in deaerated condition for 1 and 7 days. Results showed that the pH of geothermal waters is the most detrimental factor in the transformation of ɣ-Al2O3 and its protective abilities. Delaminations were found in the Coating exposed to geothermal brines with pH 4. FTIR spectra indicated a transformation of ɣ-Al2O3 to boehmite AlOOH after exposure to pH 4 and 6, and bayerite Al(OH)3 was formed after exposure to pH 8. Different Crystal structures of the hydrated Al2O3 also contribute to the stability of the coatings, observed by the SEM- EDX of the surface and cross-section of coatings. This study indicated that ɣ-Al2O3 sol-gel coating presents a promising aspect of corrosion protection in geothermal environment with a neutral pH.
Influence of Precipitating Brine Components on Materials Selection for Geothermal Applications
(2021)
Since geothermal wells are a feasible energy source to replace fossil fuel supply, many technologies have been developed to take advantage of geothermal energy. Nevertheless, service conditions in geothermal facilities are in many cases extreme in terms of corrosion due to the chemical composition of hydrothermal fluids and temperatures. Therefore, materials selection based on preliminary material qualification is essential to guarantee a secure and reliable operation of the facilities. During operation of a geothermal research facility in Groß Schönebeck copper and lead effects have been found downhole. Occurring mechanisms and measures to prevent precipitation or scaling needed to be investigated as well as potential influences of such precipitates on corrosion resistance of metallic materials used for equipment.
This contribution deals with the evaluation of the corrosion behavior of carbon steel and corrosion resistant alloys in copper and/or lead containing artificial geothermal water, simulating the conditions in the Northern German Basin.
The behavior of these materials in an artificial geothermal water obtained by electrochemical measurements and exposure tests are presented. While carbon steel exhibits precipitation and deposition, higher alloyed material shows different response to such species and a higher resistance in saline geothermal water.
Basing on these results the suitability of the investigated corrosion resistant alloy is given for use in such conditions, whereas carbon steel creates difficulties due to its susceptibility to Cu- and Pb-precipitation.
Influence of Precipitating Brine Components on Materials Selection for Geothermal Applications
(2021)
By exposure and electrochemical tests in the laboratory the Cu- and Pb-effect on corrosion behavior and performance of carbon steel and a corrosion resistant alloy could be assessed. Critical material specific properties were determined by static exposure and electrochemical tests in artificial geothermal water with high salinity and low pH, containing Cu/Pb.
It could be shown that significant Cu- resp. Pb-deposition and precipitation only occurred in combination with carbon steel. Corrosion resistant alloys (e. g. Cr- and Ni-dominated stainless steels) prevent the disturbing Cu-agglomeration resp. Pb-deposition. Therefore, they are suitable to be chosen for future design of geothermal piping system, either in massive or in cladded form. Regarding corrosion, formation of crevices with non-metallic materials shall be avoided.
So, in addition to its already known limited corrosion resistance, carbon steel shall not be used when copper or lead species are content of the geothermal brine. Otherwise precipitation and/or deposition of metallic copper resp. lead must be expected, increasing the susceptibility of clogging the piping system.
From the interactions and pitting corrosion point of view, corrosion resistant alloys (preferably Ni-rich) seem to be most favorable when selecting materials for applications in such geothermal brines.
Biodiesel (FAME) from rapeseed is an environmentally friendly alternative to common fossil fuels. It is also suitable to serve as blending component to fuels like heating oil. If the fuel composition is changed, materials compatibility must be guaranteed. Adding polar biodiesel to nonpolar heating oil, changes the blend’s solvency and might cause swelling, extraction and solvation of polymers.
The objective of this research was to investigate the compatibility of polymeric materials, which are commonly used for components in middle distillate facilities, along with blends of heating oil and 20 % biodiesel (B20). For this propose, ACM, HNBR, FKM, PE, PA 6, POM, PUR and PVC were exposed to heating oil and B20 for 42 and 84 days at 40 °C. In addition, the polymers HNBR, FKM, PA, POM and PVC were also exposed at 70 °C. Furthermore, the resistance of polymers in eight-year aged B10 at 40 °C was evaluated. Ageing of biodiesel increases acidity which might propagate polymer corrosion.
The materials were evaluated as resistant, if the loss in tensile properties (tensile strength and elongation at break) and Shore hardness remained under 15 % compared to the initial unexposed material values. For investigations under compressed conditions, the compression set was determined for specimens of ACM, FKM and HNBR after exposure in heating oil B0 and B20 for 3,7,14, 28, 56 and 90 days at 40 °C according to ISO 815-1.
It was found that the resistance in B20 at 40 °C was given for all tested polymers except PUR. In the 8 years aged B10, PUR and POM were not compatible and ACM just conditionally compatible. At 70 °C, FKM and PVC were resistant in B20, whereas HNBR and PA 6 were not compatible. Swelling occurred for the elastomers ACM, HNBR and PUR.
Biodiesel (FAME) from rapeseed is an environmentally friendly alternative to common fossil fuels. It is also suitable to serve as blending component to fuels like heating oil. If the fuel composition is changed, materials compatibility must be guaranteed. Adding polar biodiesel to nonpolar heating oil, changes the blend’s solvency and might cause swelling, extraction and solvation of polymers. The objective of this research was to investigate the compatibility of polymeric materials, which are commonly used for components in middle distillate facilities, along with blends of heating oil and 20 % biodiesel (B20). For this propose, ACM, HNBR, FKM, PE, PA 6, POM, PUR and PVC were exposed to heating oil and B20 for 42 and 84 days at 40 °C. In addition, the polymers HNBR, FKM, PA, POM and PVC were also exposed at 70 °C. Furthermore, the resistance of polymers in eight-year aged B10 at 40 °C was evaluated. Ageing of biodiesel increases acidity which might propagate polymer corrosion. The materials were evaluated as resistant, if the loss in tensile properties (tensile strength and elongation at break) and Shore hardness remained under 15 % compared to the initial unexposed material values. For investigations under compressed conditions, the compression set was determined for specimens of ACM, FKM and HNBR after exposure in heating oil B0 and B20 for 3,7,14, 28, 56 and 90 days at 40 °C according to ISO 815-1. It was found that the resistance in B20 at 40 °C was given for all tested polymers except PUR. In the 8 years aged B10, PUR and POM were not compatible and ACM just conditionally compatible. At 70 °C, FKM and PVC were resistant in B20, whereas HNBR and PA 6 were not compatible. Swelling occurred for the elastomers ACM, HNBR and PUR.
“Corrosive to Metals” (H290) describes the general potential danger of a substance to metallic materials. Uniform and localized attack is considered. It has nothing to do with containment material. Corrosion resistance of materials is determined similarly, but with much lower threshold values.
Manual shall provide a simple test to easily determine the aggressivity potential to cause corrosion on metallic materials.
Even a simple test requires experienced personnel. There seems to be a need of awareness and understanding training for both officials and applicants.
CO2 quality specifications are not only a matter of CO2 purity (i.e. CO2 content).
The “rest” also matters, in particular contents of reactive impurities affecting material corrosion (and rock alteration).
Also chemical reactions in CO2 stream needs to be considered, in particular when combining CO2 streams of different compositions.
Al2O3 coatings are often used as protective layers on steels against electrochemical and high-temperature corrosion because they are chemically inert and stable at elevated temperatures. This study presents preliminary work on the possibilities of using Al2O3 sol-gel coatings for corrosion protection of martensitic stainless steels in geothermal environments. Al2O3 sol-gel coatings were applied on UNS S42000, which is known to be susceptible to uniform and localized corrosion. The coated steel specimens were then tested in two types of artificial geothermal water, which simulate the geothermal fluids found in Sibayak (SBY), Indonesia, and North German Basin (NGB), Germany, respectively. SBY has pH 4 and 1.5 g/L of chloride ions, whereas NGB has a pH of 6 and 166 g/L of chloride ions. All experiments were carried out in autoclaves at 150 °C and 1 MPa under the deaerated condition. Evaluations were performed by investigating the surface profiles of both uncoated and coated steels before and after the corrosion test using a Laser Scanning Microscope (LSM) and Scanning Electron Microscope (SEM). Finally, Electrochemical Impedance Spectroscopy (EIS) was performed to compare the corrosion resistance of Al2O3 coated steels in SBY and NGB solutions. It was observed from the corrosion test that Al2O3 coatings are more suitable for use in the geothermal water with a higher pH.
The collaborative project “Impacts of impurities in CO2 streams captured from different emitters in a regional cluster on transport, injection and storage (CLUSTER)” aimed to set up recommendations on how to define “reasonable minimum composition thresholds” that CO2 streams should meet when accessing CO2 transport pipeline networks. Within CLUSTER, we investigated potential impacts of CO2 streams with different and temporally variable compositions and mass flow rates along the whole CCS chain. Investigations included, amongst others, impacts on: Corrosion of pipeline steel, pipeline network design and related transport costs, alteration of well bore cements, pressure development and rock integrity, geochemical reactions, and petrophysical and geomechanical rock properties.
All investigations are based on a generic CCS chain scenario. In this scenario, CO2 streams are captured from a spatial cluster of eleven emitters and collected in a regional pipeline network. Emitters comprise seven fossil fuel-fired power plants equipped with different capture technologies, two cement plants, one refinery and one integrated iron and steel plant. In total, 19.78 Mio t CO2 (including impurities) are captured in the emitter cluster annually. The combined CO2 stream is transported in a trunk line with a length of 400 km (100 km of these offshore) and is injected into five generic storage structures. The storage reservoirs are saline aquifers of the Buntsandstein.
The investigations revealed beneficial and deteriorating impacts of different impurities and combinations thereof. Overall, no fundamental technical obstacles for transporting, injecting and storing CO2 streams of the modelled variable compositions and mass flow rates were observed. Based on the results, the CLUSTER project team recommends not to define “minimum composition thresholds” for CO2 streams as strict threshold values for each individual impurity in the stream. Instead, CO2 stream compositions and variabilities for specific CCS projects should be constrained with regard to a set of parameters including i) the overall CO2 content, ii) maximum contents of relevant impurities or elements, iii) acceptable variability of CO2 stream composition, and iv) impurity combinations to be avoided.
Al2O3 coatings are often used as protective layers on steels against electrochemical and high-temperature corrosion because they are chemically inert and stable at elevated temperatures. This study presents preliminary work on the possibilities of using Al2O3 sol-gel coatings for corrosion protection of martensitic stainless steels in geothermal environments. Al2O3 sol-gel coatings were applied on UNS S42000, which is known to be susceptible to uniform and localized corrosion. The coated steel specimens were then tested in two types of artificial geothermal water, which simulate the geothermal fluids found in Sibayak (SBY), Indonesia, and North German Basin (NGB), Germany, respectively. SBY has pH 4 and 1.5 g/L of chloride ions, whereas NGB has a pH of 6 and 166 g/L of chloride ions. All experiments were carried out in autoclaves at 150 °C and 1 MPa under the deaerated condition. Evaluations were performed by investigating the surface profiles of both uncoated and coated steels before and after the corrosion test using a Laser Scanning Microscope (LSM) and Scanning Electron Microscope (SEM). Finally, Electrochemical Impedance Spectroscopy (EIS) was performed to compare the corrosion resistance of Al2O3 coated steels in SBY and NGB solutions. It was observed from the corrosion test that Al2O3 coatings are more suitable for use in the geothermal water with a higher pH.
The collaborative project “Impacts of impurities in CO2 streams captured from different emitters in a regional cluster on transport, injection and storage (CLUSTER)” aimed to set up recommendations on how to define “reasonable minimum composition thresholds” that CO2 streams should meet when accessing CO2 transport pipeline networks. Within CLUSTER, we investigated potential impacts of CO2 streams with different and temporally variable compositions and mass flow rates along the whole CCS chain. Investigations included, amongst others, impacts on:
• corrosion of pipeline steel,
• pipeline network design and related transport costs,
• alteration of well bore cements,
• pressure development and rock integrity,
• geochemical reactions, and
• petrophysical and geomechanical rock properties.
All investigations are based on a generic CCS chain scenario. In this scenario, CO2 streams are captured from a spatial cluster of eleven emitters and collected in a regional pipeline network. Emitters comprise seven fossil fuel-fired power plants equipped with different capture technologies, two cement plants, one refinery and one integrated iron and steel plant. In total, 19.78 Mio t CO2 (including impurities) are captured in the emitter cluster annually. The combined CO2 stream is transported in a trunk line with a length of 400 km (100 km of these offshore) and is injected into five generic storage structures. The storage reservoirs are saline aquifers of the Buntsandstein.
The investigations revealed beneficial and deteriorating impacts of different impurities and combinations thereof. Overall, no fundamental technical obstacles for transporting, injecting and storing CO2 streams of the modelled variable compositions and mass flow rates were observed. Based on the results, the CLUSTER project team recommends not to define “minimum composition thresholds” for CO2 streams as strict threshold values for each individual impurity in the stream. Instead, CO2 stream compositions and variabilities for specific CCS projects should be constrained with regard to a set of parameters including i) the overall CO2 content, ii) maximum contents of relevant impurities or elements, iii) acceptable variability of CO2 stream composition, and iv) impurity combinations to be avoided.
Study of Polyaniline/Silicon Dioxide based Coating on Carbon Steel in Artificial Geothermal Brine
(2021)
Geothermal brines are corrosive in nature because of their salt contents and high temperatures. Therefore, they pose a major challenge to geothermal power-plants, which are mostly built of low alloyed steels, e.g., carbon steel. Carbon steel is susceptible to uniform and localized corrosion when exposed to geothermal brines having acidic-saline properties. To overcome this limitation, geothermal power plants should be built by either high alloyed materials or by integrating protection systems on carbon steel, such as coatings and inhibitors. We studied a coating system containing polyaniline/silicon dioxide basing on locally available resources that provides protection against corrosion of carbon steel and enhance the thermal resistance in geothermal environments. Here, exposure and electrochemical tests of coated carbon steels were performed in an artificial geothermal brine. The solution had a pH of 4, with the composition of 1,500 mg/L of chlorides, which is based on the chemical analysis of geothermal brine found in Sibayak, Indonesia. All exposure tests were conducted using autoclaves at 150 °C with a total pressure of 1 MPa, which was performed for up to six months to evaluate the durability of the coating system. Post-experimental analyses were performed by assessing the surface of specimens using optical and electron microscopes. On the other hand, electrochemical tests were performed for seven days at 25 °C and 150 °C to investigate the kinetics of electrochemical reactions by measuring open circuit potential and electrochemical impedance spectra. Experimental results showed the corrosion resistance of PANI/SiO2 composite coatings, where polyaniline and SiO2 play their roles as stabilizers.
Study of Polyaniline/Silicon Dioxide based Coating on Carbon Steel in Artificial Geothermal Brine
(2021)
By using the available resources in Indonesia, such as silicon dioxide and marine coating base, the PANI/SiO2 modified alkyd coating was able to protect carbon steel in a deaerated artificial geothermal water. The screening of coatings shows that the modification by adding individual pigment was not sufficient to protect carbon steel even during a short-term exposure, indicated by the discoloration after only seven days of exposure. Electrochemical tests indicated that there was no significant change in the Ecorr between the coated and uncoated carbon steel at room temperature. At 150 °C, the coated carbon steel has a lower potential than that of carbon steel, indicating that the coating is protecting carbon steel cathodically or slowing down the corrosion reaction. Finally, a long-term exposure test confirmed that the PANI/SiO2 modified coating successfully protects the carbon steel in the Sibayak artificial geothermal water up to 150 °C for 6 months.
Im DGMK-Projekt 780 wurde eine forcierte Prüfmethode entwickelt zur Bestimmung der Beständigkeit von metallenen Werkstoffen gegenüber Brennstoffen aus Mitteldestillaten und Gemischen aus Mitteldestillat und paraffinischen Kohlenwasserstoffen, die jeweils Fettsäuremethylester (FAME) als biogene Komponente enthalten. Bei der Prüfmethode werden Proben des Werkstoffes in einem speziellen Prüfmedien ausgelagert. Die Zusammensetzung von zwei Prüfmedien wurde im Vorhaben erarbeitet. Die Prüfmedien decken für den FAME-Anteil einen Bereich von bis zu 20 % (V/V) ab. Die Auslagerung kann bei geringem Aufwand unter Atmosphärendruck durchgeführt werden.
Die Eignung einer Auswahl von metallenen Werkstoffen und Polymerwerkstoffen, die für Versorgungsanlagen für Mitteldestillat relevant sind, wurde durch Auslagerung in folgenden nicht gealterten Brennstoffen bestimmt: Heizöl EL schwefelarm (B0), Heizöl EL schwefelarm mit 20 % (V/V) FAME (B20), FAME (B100) und hydriertes Pflanzenöl (HVO). Die Temperatur bei der Auslagerung betrug 50 °C für die metallenen Werkstoffe und 40 °C und 70 °C für die Polymerwerkstoffe. Die Ergebnisse der Beständigkeitsbewertung wurden in Beständigkeitslisten zusammengefasst. Die mit dem B20 erhaltenen Werkstoffbeständigkeiten gelten generell für Gemische aus Heizöl EL schwefelarm und FAME mit einem FAME-Gehalt bis zu 20 % (V/V). Sie sind auch auf Gemische aus Dieselkraftstoff und FAME mit einem FAME-Gehalt bis 20 %(V/V) übertragbar.
Die forcierte Prüfmethode kann insbesondere KMUs bei der Weiterentwicklung von bestehenden Produkten und der Entwicklung von neuen Produkten als ein kostengünstiger Schnelltest zur Überprüfung der Werkstoff- und Bauteilbeständigkeit gegenüber Mitteldestillaten mit hohem FAME-Anteil dienen. Sie kann für die Hersteller die Sicherheit erhöhen, dass Bauteile die Freigabeprüfungen der Bauaufsicht bestehen, wobei die Freigabe aber nur für Deutschland gültig ist.
Die Erkenntnisse des Forschungsvorhabens können in eine harmonisierte Europäischen Norm für alternative Brenn- und Kraftstoffe einfließen. Diese ist für die Bauteilhersteller die Voraussetzung für die Erschließung des europäischen Marktes.
Im Vorhaben wurde eine forcierte Prüfmethode zur Bestimmung der Beständigkeit von metallenen Werkstoffen gegenüber Brennstoffen aus Mitteldestillaten und Gemischen aus Mitteldestillat und paraffinischen Kohlenwasserstoffen, die jeweils Fettsäuremethylester (FAME) als biogene Komponente enthalten, entwickelt. Bei der Prüfmethode werden Prüfkörper des jeweiligen Werkstoffes in speziellen Prüfmedien ausgelagert. Die Zusammensetzung von zwei Prüfmedien wurde im Vorhaben erarbeitet. Diese Prüfmedien erfassen die Effekte der Alterung des FAME, die zu erwarten sind, wenn der Brennstoff länger als 2 Jahre im Feld lagert. Sie decken den Bereich bis 20 % (V/V) FAME-Anteil ab. Die Auslagerung kann bei geringem Aufwand unter Atmosphärendruck durchgeführt werden.
Die Eignung einer Auswahl von metallenen Werkstoffen und Polymerwerkstoffen, die für Versorgungsanlagen für Mitteldestillat relevant sind, wurde durch Auslagerung in folgenden nicht gealterten Brennstoffen bestimmt: Heizöl EL schwefelarm (B0), Heizöl EL schwefelarm mit 20 % (V/V) FAME (B20), FAME (B100) und hydriertes Pflanzenöl (HVO). Die Werkstoffe wurden auch in einem 1 Jahr gealterten B20 und einem 8 Jahre gealtertem B10 ausgelagert. Die Temperatur bei der Auslagerung betrug 50 °C für die metallenen Werkstoffe und 40 °C und 70 °C für die Polymerwerkstoffe. Die Ergebnisse der Beständigkeitsbewertung wurden in Beständigkeitslisten zusammengefasst. Die mit B20 erhaltenen Bewertungen gelten generell für Gemische aus Heizöl EL schwefelarm und FAME mit einem FAME-Gehalt bis 20 % (V/V). Sie sind auch auf Gemische aus Dieselkraftstoff und FAME mit einem FAME-Gehalt bis 20 %(V/V) übertragbar.
Die forcierte Prüfmethode kann insbesondere KMUs bei der Weiterentwicklung von bestehenden Produkten und der Entwicklung von neuen Produkten als ein kostengünstiger Schnelltest zur Überprüfung der Werkstoff- und Bauteilbeständigkeit gegenüber Mitteldestillaten mit hohem FAME-Anteil dienen. Sie kann für die Hersteller die Sicherheit erhöhen, dass Bauteile die Freigabeprüfungen der Bauaufsicht bestehen, wobei die Freigabe jedoch nur für Deutschland gültig ist.
Die Erkenntnisse des Forschungsvorhabens können in eine harmonisierte Europäische Norm für alternative Brenn- und Kraftstoffe einfließen. Diese ist für die Bauteilhersteller die Voraussetzung für die Erschließung des europäischen Marktes.
Die Werkstoffklasse der Nichteisenmetalle gewinnt wegen ihrer unzähligen Anwendungsmöglichkeiten nicht nur im Maschinen‐ und Anlagenbau eine immer größere technische und wirtschaftliche Bedeutung, sodass es unabdingbar ist, insbesondere Studierenden der Material‐ und Werkstoffwissenschaften und des Maschinenbaus, den aktuellen Wissensstand auf diesem Gebiet zu vermitteln. Mit dieser Neuerscheinung veröffentlicht der Wiley‐VCH‐Verlag ein solches Lehrbuch. Kompakt und übersichtlich machen die beiden Autoren den Leser in 10 Kapiteln auf verständliche Art mit dieser Thematik vertraut. Dabei kommt ihnen ihre durch langjährige Lehrtätigkeit erworbene didaktische Erfahrung sehr zugute.
Alles in allem bietet dieses Lehrbuch durch seinen von den Natur‐, über Material‐ zu Ingenieurwissenschaften weitgespannten Bogen einen interessanten und übersichtlichen Einstieg in die Welt der am häufigsten verwendeten Nichteisenmetalle, wobei es keinen Anspruch auf Vollständigkeit erhebt.
Indonesien gilt aufgrund seiner vielen Vulkane als einer der Hotspots für Geothermie. Doch Salz und Hitze setzen den Geothermie‐Anlagen zu und gefährden ihre Sicherheit und Wirtschaftlichkeit. Ein Team an der BAM hat günstigen, lokal verfügbaren Baustahl jetzt so beschichtet, dass ein nachhaltiger und sicherer Betrieb der Geothermie‐Kraftwerke möglich ist ‐ auch unter Extrembedingungen.
Das BAM‐Team will das Beschichtungssystem nun den Anwendern in Indonesien zur Verfügung stellen, damit es unter Realbedingungen in einem Geothermie‐Kraftwerk getestet werden kann. Der Schutz vor Korrosion ist mitentscheidend, weil sie die Lebensdauer dieser Kraftwerke bestimmt. Unsere Arbeit könnte die Effizienz der Energieproduktion mit Geothermie wesentlich verbessern.
This book introduces to aspects to be considered when dealing with coatings and linings. Philip A. Schweitzer covers and compares a variety of specific coatings and their applications. In 18 chapters he divided the content into two main parts: linings and coatings.
All professionals involved in design and maintenance processes get by this book a compact survey of necessary considerations which needs to be done when applying surface protection measures. The literature references at the end of some chapters support the readers finding additional information about the special topic, mainly written by the author himself. Since this newly issued paperback edition is a 1:1 re‐print of the 2001 hardcover version, neither current publications are referenced, nor revisions were made.
Das 1988 erstmalig erschienene und bewährte Fachbuch wurde auf den neuesten Stand gebracht und im Rahmen der „Kontakt & Studium“‐Serie der Technischen Akademie Esslingen als Band 243 neu aufgelegt.
In 12 Kapiteln bieten die 12 erfahrenen Autoren einen Überblick über die gebräuchlichsten Formen zerstörungsfreier Prüfverfahren als Grundlage für die Dokumentation der Produktqualität während des gesamten Herstellungsprozesses und deren elementare Bedeutung für die Produkthaftung.
Dieses Lehrbuch dient nicht nur Universitäts‐Studierenden, sondern bietet auch jedem interessierten Leser einen Überblick der gebräuchlichen Verfahren.
The first edition of this book, published within the series “Materials Science – Metals and Alloys”, provides broad knowledge of this interesting and widely applied metal from manufacturing and production to finishing and application in 13 chapters, written by 29 contributors. Each chapter is separately concluded and ends with references used.
This book fulfills its intention of conveying comprehensive and cutting‐edge knowledge of magnesium alloys. It is useful for practicing engineers, researchers and students searching for an instructional and reference source.
his fully updated examination of sustainable processes for gaseous and liquid biofuels production, published for the second time within the series “Biomass, Biofuels, Biochemicals”, provides 33 contributions made by 120 authors. They present a holistic view of biofuels in research, operation, scale‐up and application. Comparing to the first edition, all chapters have been updated and new chapters covering topics of current interest, including sustainability and biohydrogen have been added.
By its wide overview on existing technologies, this book provides state‐of‐the‐art information and knowledge to the desired readership, like post‐graduates, researchers in the area of biofuels, wastewater treatment, alternate energy sources, renewable energy from biomass, chemical and biochemical engineers, microbiologists, biotechnologists working in academic and research institutes as well as in industry and governmental agencies.
Die von Stephan W. Koch herausgegebene Übersetzung der erweiterten zehnten Auflage von ,,Fundamentals of Physics“ liefert ein Schwergewicht geballten Physikwissens und Übungsmaterial. Die Bücher bieten nicht nur Studierenden hilfreiches Lernmaterial, sondern sind auch für allgemein Physik‐Interessierte ein wertvolles Nachschlagewerk. Wer sich bereits mit dem umfassenderen „großen Bruder“ vertraut gemacht hat und diesen nutzt, findet im Lehrbuch nichts Neues. Jedoch liefert das Übungsbuch im Vergleich zum Arbeitsbuch von 2018 neue und übersichtlichere Übungsbeispiele.
Die neue Auflage wurde didaktisch komplett neu strukturiert und einige Kapitel vollständig überarbeitet. Ein Novum stellt dabei die modulare Organisation dar, bei der jeder Abschnitt mit Lernzielen und Schlüsselideen beginnt. Kontrollfragen im Text tragen entscheidend zum Rekapitulieren des Gelesenen bei. Jedes Kapitel endet mit einer Zusammenfassung und Fragen zum vermittelten Stoff. Als Ergänzung dient das ausführliche Übungsbuch mit Aufgaben und Lösungen zu den jeweiligen Kapiteln des Lehrbuches.
Die 37 Kapitel machen verständlich mit den einzelnen Gebieten der Physik vertraut.
Since geothermal wells are a feasible energy source to replace fossil fuel supply, many technologies have been developed to take advantage of geothermal energy. Nevertheless, service conditions in geothermal facilities are in many cases extreme in terms of corrosion due to the chemical composition of hydrothermal fluids and temperatures. Therefore, materials selection based on preliminary material qualification is essential to guarantee a secure and reliable operation of the facilities. During operation of a geothermal research facility in Groß Schönebeck copper and lead effects have been found downhole. Occurring mechanisms and measures to prevent precipitation or scaling needed to be investigated as well as potential influences of such precipitates on corrosion resistance of metallic materials used for equipment.
This contribution deals with the evaluation of the corrosion behavior of carbon steel and corrosion resistant alloys in copper and/or lead containing artificial geothermal water, simulating the conditions in the Northern German Basin.
The behavior of these materials in an artificial geothermal water obtained by electrochemical measurements and exposure tests are presented. While carbon steel exhibits precipitation and deposition, higher alloyed material shows different response to such species and a higher resistance in saline geothermal water.
Basing on these results the suitability of the investigated corrosion resistant alloy is given for use in such conditions, whereas carbon steel creates difficulties due to its susceptibility to Cu- and Pb-precipitation.
This paperback issue of the 2007 hardcover version within the “Corrosion Engineering Handbook” series presents various materials and methods for controlling and protecting against corrosion instead of using expensive alloys to construct a tank or processing vessel.
This book is a very comprehensive collection of the current knowledge about applied linings and coatings. So, it fulfills its intension, “that regardless of what is being built, … information for … whoever is responsible for the selection of material of construction will be found in this book to enable them to avoid unnecessary loss of material through corrosion”, to a very large extent.
This book by Scrivener Publishing contains 14 chapters written by 82 leading scientists, experienced in the field of coatings. They demonstrate mechanisms, usage and manipulation of cutting‐edge coating methods. Each chapter is well structured and ends with a conclusion, highlighting the content. The book is divided into 3 parts: “Materials and Methods”, “Coating Materials Nanotechnology” and “Advanced Coating Technology and Applications”.
Finally, this book provides a comprehensive insight into innovative research in advanced coating materials and state‐of‐the‐art technologies, without being a real textbook. It fulfills its intension of being beneficial both for technicians and scientists.
Since nanoscience has a tremendous impact on the development of electrochemistry, Wiley‐VCH paid attention to that by publishing thisbook as volume 17 within the series “Advances in Electrochemical Science and Engineering”.
This collection of “nanoaspects”on electrodes provides a helpful overview on principles and current findings to readers interested in such applications. It fulfills its intention of being “a valuable resource for researchers working in such fields as electrochemistry, materials science, spectroscopy, analytical and medicinal chemistry”.
This book grew out of a course on polymer coatings held by the author at the university. It shall serve as an introduction to the wide field of polymer coatings. It is not intended to cover completely all facts on polymer coatings.
All chapters are well structured. Selected figures and formulas illustrate the content and contribute to a good understandability. At the end of each chapter some hints for further reading are provided.
Finally, the book fulfills its intention to introduce into the topic by providing basics on science and technology of polymer coatings, suitable for chemists in industry, materials scientists, polymer chemists and physical chemists.
This concise reference book,consisting of 2 volumes, provides “key scientific and technical properties and data” for “materials scientists, metallurgists, engineers,chemists, and physicists as well as academic staff, technicians, and students” dealing with such kind of materials.
Within its 3rd edition the previous work was extended by a chapter on occupational health and safety issues of materials, beside of the update of whole content. Within 22 chapters materials properties and data are summarized in many tables. Some facts are illustrated by drawings and diagrams for better understandability. Each chapter ends with a part on further reading arranged accordingly.
Rezension: Kurzlehrbuch Physikalische Chemie: für natur‐ und ingenieurwissenschaftliche Studiengänge
(2020)
Wem das Standardwerk der Physikalischen Chemie „Der Atkins“ zunächst zu überwältigend erscheint, dem gelingt mit diesem, nunmehr in der fünften Auflage erschienenen, Kurzlehrbuch sicherlich der Einstig in die Thematik. Studierenden im Bachelor‐ und Mastergang bietet es ein sehr hilfreiches Nachschlagewerk während des Studiums und zur Prüfungsvorbereitung. Die vielfältigen Übungen und Anwendungen am Ende jedes Kapitels, besser gesagt von jedem Fokus, tragen entscheidend zum Verständnis und Überprüfen des Gelernten bei. Sogenannte „Toolkits“ wiederholen an den entsprechenden Stellen inprägnanter Form mathematische Herangehensweisen und Techniken, die das Textverständnis unterstützen. Bei der Überarbeitung der vorherigen Ausgabe flossen nicht nur Anmerkungen von Lehrenden, sondern auch wertvolle Einblicke aus der Sicht der Lernenden, ein, was sich im Aufbau des Buches widerspiegelt.
Dieses didaktisch und inhaltlich sehr gut aufgebaute Lehrbuch erfüllt auf jeden Fall seine Intension und weckt die Neugierde auf das im Frühjahr 2020 erscheinende dazugehörige Arbeitsbuch.
This edition, published as first issue within the series “Corrosion Atlas”, provides 181 corrosion case studies, collected from 29 contributors.
These Corrosion Atlas Case Studies provide a helpful tool required for engineers in their daily life to quickly determine and solve their equipment's corrosion problems by compact theoretical background and vivid examples. It fulfills the intension of the editors to be “the first centralized collection of case studies containing challenges paired directly with solutions together in one location”.
Polymere sind aus unserem Alltag nicht mehr wegzudenken. Häufig haben wir mit Plexiglas, Dichtmassen, Klebestreifen und vielen Verpackungsmaterialien zu tun. Aber auch Spezialanwendungen (z.B. in der Pharmazie) bilden Einsatzbereiche dieser Werkstoffe.
Der Vermittlung der Grundlagen polymerer Werkstoffe in den Studienfächern Chemie, Materialwissenschaften und der Ingenieur‐ und Lebenswissenschaften haben sich die Autoren verschrieben, wobei sie zur verständlichen Anschauung bewusst auf das Beispiel Styrol als „Versuchskaninchen“ zurückgreifen.
Dieses Lehrbuch wird seinem Anspruch gerecht, einen leichten Einstieg in die Polymerwissenschaften zu ermöglichen. Es liefert eine Übersicht über die Polymerklassen Thermoplaste, Duroplaste und Elastomere mit ihren Eigenschaften und zeigt, welche Synthesestrategie zu dem Produkt mit den gewünschten Eigenschaften führt. Anhand von Beispielen aus dem Alltag werden gängige Vertreter verständlich vorgestellt.
Currently, storage of electric energy is becoming more and more interesting in terms of applicability and efficiency. One way is the electrochemical storage by already well‐developed battery‐systems. This textbook provides an introduction into physical and chemical processes necessary for battery application.
This book fulfills its intension to serve graduate students of electrical engineering as an introduction into the field of batteries. Even students and interested readers of other faculties might find an introduction in physical and chemical background of batteries.
The aim of the work presented was the evaluation of corrosion resistance
of various materials in geothermal Waters as a base to create a catalogue of suitable materials for applications in (not only) German geothermal power plants.
Users shall be enabled to have a basis for designing such facilities. High alloyed corrosion resistant alloys are suitable and do not cause copper or lead deposition. They shall be chosen for future design of the piping system, either in massive or in cladded form, if crevices formation with non-metallic materials can be prevented!
Schlosserei‐, Metall‐ und Stahlbaubetriebe müssen seit Juli 2012 für tragende Bauteile aus Stahl und Aluminium, die als Bauprodukte in Verkehr gebracht werden sollen, einen Konformitätsnachweis nach DIN EN 1090‐1 erbringen.
Mit der sechsten Auflage des Normen‐Handbuches „Schweißen im Stahlbau“ setzen das Deutsche Institut für Normung e.V. (DIN) und der Deutsche Verband für Schweißen und verwandte Verfahren e.V. (DVS) ihre bewährte Strategie fort, die dieses Thema betreffenden aktuellen Normen und Regelwerke durch J. W. Mußmann in gut aufbereiteter Form kompakt zusammenzustellen.
Since data processing has now also found its way into materials science, there has been a great demand from users for a corresponding textbook. This book provides a guide to the latest advances of materials informatics and data mining for materials science. 46 authors introduce readers to methods, present tools and case studies to illustrate the power of materials informatics within this new field of application.
Often 3D‐printing and additive manufacturing are mentioned as the 3rd industrial revolution. In this conjunction this book provides a brief overview on additively manufactured metal pieces.
This book fulfills its intension to serve as an educational guide, providing a holistic picture encompassing science, technology and applications for the real‐life use of Metal Additive Manufacturing.
This contribution provides current findings regarding materials susceptibility for CCUS applications. Basing on results gathered in 2 German long-term projects (COORAL and CLUSTER) suitable materials are introduced as well as dominating impurities of the CO2 stream and corrosion mechanisms. Investigations cover the whole CCUS process chain and provide the following recommendations for certain parts. Commercially available carbon steels are suitable for compression and pipelines as long as moisture content and impurities are limited (water 50 to 100 ppmv, SO2 and NO2 ca. 100 ppmv).
Corrosion rates increase with increasing water content (0.2 – 20 mm/a).
Condensation of acids and therefore droplet formation is always possible, even at low water contents.
A low SO2 content within the CO2-stream might be more important than a low water content.
Cr13-steels showed a general susceptibility to shallow pitting and pitting. So, they seem to be not suitable for CCUS applications.
Low alloyed steels showed better corrosion behavior (predictable uniform corrosion).
For direct contact with saline aquifer fluids only high alloyed steels shall be used.