In corrosive environments such as CCS bore holes or geothermal power plants the materials loaded cyclically are also exposed constantly to the highly corrosive hot thermal water. The lifetime reduction of (X46Cr13, AISI 420C) is demonstrated in in-situ-laboratory experiments (T=60 °C, geothermal brine: Stuttgart Aquifer flow rate: 9 Nl/h, CO2). S-N plots, micrographic-, phase-, fractographic- and surface analysis were applied to obtain sustainable information on the corrosion fatigue behavior. Maximum number of cycles (here 12.5 x 106 cycles to failure) is reached at σa =173 MPa. No typical fatigue strength exists and passive corrosion fatigue is most likely failure cause.