The formation of laser-induced periodic surface structures (LIPSS) upon irradiation of fused silica with multiple irradiation sequences of parallel polarized Ti:sapphire femtosecond laser pulse pairs (160 fs pulse duration, 800 nm central wavelength) was studied experimentally. For that purpose, a Michelson interferometer was used to generate near-equal-energy double-pulse sequences allowing the temporal pulse delay between the parallel-polarized individual fs-laser pulses to be varied between 0 and 40 ps with ~0.2 ps temporal resolution. The surface morphologies of the irradiated surface areas were characterized by means of scanning electron and scanning force microscopy. In the sub-ps delay range a strong decrease of the LIPSS periods and the ablation crater depths with the double-pulse delay was observed indicating the importance of the laser-induced free-electron plasma in the conduction band of the solids for the formation of LIPSS.
The formation of laser-induced periodic surface structures (LIPSS) upon irradiation of fused silica with multiple irradiation sequences consisting of five Ti:sapphire femtosecond (fs) laser pulse pairs (150 fs, 800 nm) is studied experimentally. A Michelson interferometer is used to generate near-equal-energy double-pulse sequences with a temporal pulse delay from -20 to +20 ps between the cross-polarized individual fs-laser pulses (~0.2 ps resolution). The results of multiple double-pulse irradiation sequences are characterized by means of Scanning Electron and Scanning Force Microscopy. Specifically in the sub-ps delay domain striking differences in the surface morphologies can be observed, indicating the importance of the laser-induced free-electron plasma in the conduction band of the solids for the formation of LIPSS.
The formation of laser-induced periodic surface structures (LIPSS) upon irradiation of fused silica and silicon with multiple (NDPS) irradiation sequences consisting of linearly polarized femtosecond laser pulse pairs (pulse duration ~150 fs, central wavelength ~800 nm) is studied experimentally. Nearly equal-energy double-pulse sequences are generated allowing the temporal pulse delay Δt between the cross-polarized individual fs-laser pulses to be varied from -40 ps to +40 ps with a resolution of ~0.2 ps. The surface morphologies of the irradiated surface areas are characterized by means of scanning electron and scanning force microscopy. Particularly for dielectrics in the sub-ps delay range striking differences in the orientation and spatial characteristics of the LIPSS can be observed. For fused silica, a significant decrease of the LIPSS spatial periods from ~790 nm towards ~550 nm is demonstrated for delay changes of less than ~2 ps. In contrast, for silicon under similar irradiation conditions, the LIPSS periods remain constant (~760 nm) for delays up to 40 ps. The results prove the impact of laser-induced electrons in the conduction band of the solid and associated transient changes of the optical properties on fs-LIPSS formation.
The formation of laser-induced periodic surface structures (LIPSS) on different materials (silicon, fused silica, quartz) with linearly polarized fs-laser irradiation is studied experimentally. In dielectrics, the importance of transient excitation stages in the LIPSS formation is demonstrated by using (multiple) cross-polarized double-fs-laser-pulse irradiation sequences. A characteristic decrease of the spatial LIPSS periods is observed for double-pulse delays of less than 2 ps along with a characteristic 90°-rotation of the LIPSS orientation.