It has been successfully demonstrated that ceramic materials can be joined in the green
state without a second phase by using low pressure injection molded parts. The investigation of the
joining interface revealed that a high quality interface can be achieved by carefully adjusting the
different manufacturing steps. The use of monomodal particle size distribution in the used powder
CT3000SG is inferior to a broader particle size distribution obtained by replacing 33% of the finer
alumina powder by coarser CT1200SG. In this way the dewaxing process is significantly improved
when the wall thickness of the part exceeds 3 mm. The investigation of the mechanical properties of
the joined and sintered parts revealed, that the bending strength of the joined specimens achieved
about 80 % of the unjoined, monolithic specimens.
The surface of a titanium alloy (Ti6Al4V) implant material was covered with a bioactive calcium alkali phosphate ceramic with the aim to accelerate the healing and to form a stronger bond to living bone tissue. To fix the ceramic powder we used a femtosecond laser, which causes a thin surface melting of the metal. It is a requirement to prove that the laser irradiation would not reduce the lifetime of implants. Here we present the results of mechanical stability tests, determined by the rotating bending fatigue strength of sample rods. After describing the sample surfaces and their modifications caused by the laser treatment we give evidence for an unchanged mechanical stability. This applies not only to the ceramic fixation but also to a comparatively strong laser ablation.