TY - CONF A1 - Woydt, Mathias A1 - Mohrbacher, H. T1 - The tribological property profile of hard metals and metal matrix composites based on niobium carbide T2 - Proceedings of the International Symposium on Wear Resistant Alloys for the Mining and Processing Industry N2 - This work is focused on the tribological profile of NbC-based material, as well as their potential applications and environmental implications. T2 - International Symposium on Wear Resistant Alloys for the Mining and Processing Industry CY - Sao Paulo, Brazil DA - 04.05.2015 KW - Niobium carbide KW - Metal KW - Binder KW - Metal matrix composite KW - Friction KW - Wear KW - Hardness KW - Solubility KW - Toughness KW - Abrasion PY - 2018 SN - 978-0-692-05382-9 SP - 427 EP - 461 AN - OPUS4-44201 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Huang, S. G. A1 - Vleugels, J. A1 - Mohrbacher, H. A1 - Woydt, Mathias T1 - NbC-based cermets: influence of secondary carbide addition and metal binder T2 - Proceedings of the International Symposium on Wear Resistant Alloy for the Mining and Processing Industry N2 - Full densification of Fe, Co and Ni bonded NbC based cermet’s was achieved by pressure less liquid phase sintering in vacuum for one hour at 1420°C. The hardness and toughness of the NbC matrix cermet’s can be mainly tailored by the binder composition and secondary carbide additions. Ni binder based NbC cermet’s allow the combination of high hardness and improved toughness. The addition of lesser amounts of VC/Cr3C2 in a NbC partially substituted WC-Co cemented carbide increased significantly the hardness in combination with a moderate fracture toughness. T2 - International Symposium on Wear Resistant Alloys for the Mining and Processing Industry CY - Sao Paulo, Brazil DA - 04.05.2015 KW - Niobium carbide KW - Hardmetal KW - Cemented carbide KW - Sintering KW - Grain growth KW - Microstructure KW - Hardness KW - Fracture toughness PY - 2018 SN - 978-0-692-05382-9 SP - 521 EP - 534 AN - OPUS4-44206 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Le Quilliec, G. A1 - Leroy, R. A1 - Richard, C. A1 - Woydt, Mathias A1 - Morandeau, A. T1 - Comparison of the life-span of NbC-Co and WC-Co inserts during different machining operations on 100Cr6 (SAE 52100) bearing steel T2 - Proceedings of the International Symposium on Wear Resistant Alloy for the Mining and Processing Industry N2 - The aim of the study presented in this paper is to highlight the potential of niobium carbide cutting tool inserts for machining and to compare their performance to commercially available tungsten carbide inserts. In this work, a comparison between a conventional Wc-Co insert and NbC-Co inserts was carried out under hard machining conditions on specimens made of 100Cr6 bearing steel grade (SAE 52100). T2 - International Symposium on Wear Resistant Alloys for the Mining and Processing Industry CY - Sao Paulo, Brazil DA - 04.05.2015 KW - Niobium carbide KW - Cobalt KW - Fe3Al KW - Inserts KW - Cutting tools KW - Wear KW - Turning PY - 2018 SN - 978-0-692-05382-9 SP - 535 EP - 545 AN - OPUS4-44207 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Genga, R. M. A1 - Cornish, L. A. A1 - Woydt, Mathias A1 - Sobiyi, K. A1 - Polese, C. T1 - Wear and Mechanical properties of spark plasma and liquid phase sintered WC and NbC based cemented carbide inserts T2 - Proceedings of the International Symposium on Wear Resistant Alloy for the Mining and Processing Industry N2 - The effects on the mechanical properties, thermal behavior, response to cutting forces and wear mechanisms have been investigated for different manufacturing processes and materials for cemented carbide inserts. T2 - International Symposium on Wear Resistant Alloys for the Mining and Processing Industry CY - Sao Paulo, Brazil DA - 04.05.2015 KW - WC KW - NbC KW - SPS KW - Co KW - Fe3Al KW - Hard-turning KW - Interrupted milling KW - Flank KW - Wear KW - Coolant-free KW - Crater wear KW - Machinability PY - 2018 SN - 978-0-692-05382-9 SP - 547 EP - 567 AN - OPUS4-44208 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Woydt, Mathias A1 - Wäsche, Rolf A1 - Brandt, Guido A1 - Ehrke, Roman A1 - Yano, S. A1 - Sasaki, S. T1 - Tribology in hot steam for energy recovery T2 - Industrial and Automotive Lubrication N2 - The wear rates of self-mated alumina couples show that friction as well as wear is largely determined by the above-mentioned hydro-thermal conditions. The presence of water and its amount available in the surrounding system either in liquid or in gaseous form plays a key role for friction and wear behavior and can be beneficial for the tribological profile of steam degradation resistant materials. Hot steam enhances the tribo-chemical formations of oxides and hydroxides on MgO-ZrO2 alumina and antimony impregnated carbon. T2 - 21th International Colloquium Tribology CY - Stuttgart/Ostfildern, Germany DA - 09.01.2018 KW - Tribology KW - Friction KW - Alumina KW - Hot steam PY - 2018 SP - 1 EP - 2 AN - OPUS4-43896 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Gradt, Thomas A1 - Theiler, Géraldine T1 - Tribological properties of polymer composites for applications in LNG environment T2 - Industrial and Automotive Lubrication N2 - In a first test series, the friction and wear properties of 6 polymeric candidate materials for application in LNG tribosystems were tested. The most favorable properties showed PTFE composite, filled with carbon fibers and PEEK, which showed low and stable friction and a wear coefficient in the order of 10-7 mm3N-1m-1. PTFE containing PEEK composites seem to be also appropriate for LNG applications. Admixtures of graphite as solid lubricant result in lower wear. Contrary, a lubricating mechanism of MoS2 was not observed. The PI-materials showed comparatively high friction and medium wear. T2 - 21th International Colloquium Tribology CY - Stuttgart/Ostfildern, Germany DA - 09.01.2018 KW - Tribology KW - PEEK KW - PTFE composites KW - Friction PY - 2018 SP - 1 EP - 2 AN - OPUS4-43900 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Theiler, Géraldine A1 - Gradt, Thomas T1 - Friction and wear characteristics of polymers in gaseous and liquid hydrogen T2 - Industrial and Automotive Lubrication N2 - The tribological characteristics of pure and graphite filled polymers were investigated in gaseous hydrogen at ambient temperatures and in LH2 at -253°C. It could be shown that the tribological properties of PI and PEEK materials is related to the formation of a transfer film. The influence of both hydrogen and cryogenic temperatures will be discussed in the presentation. T2 - 21th International Colloquium Tribology CY - Stuttgart/Ostfildern, Germany DA - 09.11.2018 KW - Friction KW - Wear KW - Hydrogen KW - PEEK PY - 2018 SP - 1 EP - 2 AN - OPUS4-43903 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Thiede, Tobias A1 - Cabeza, Sandra A1 - Mishurova, Tatiana A1 - Nadammal, Naresh A1 - Kromm, Arne A1 - Bode, Johannes A1 - Haberland, C. A1 - Bruno, Giovanni T1 - An assessment of bulk residual stress in selective laser melted Inconel 718 T2 - Proceedings ECNDT2018 N2 - Additive Manufacturing (AM) of metals has become industrially viable for a large variety of applications, including aerospace, automotive and medicine. Powder bed techniques such as Selective Laser Melting (SLM) based on layer-by-layer deposition and laser melt enable numerous degrees of freedom for the geometrical design. Developing during the manufacturing process, residual stresses may limit the application of SLM parts by reducing the load bearing capacity as well as induce unwanted distortion depending on the boundary conditions specified in manufacturing. The residual stress distribution in the bulk of IN718 elongated prisms produced by SLM was studied non-destructively by means of neutron diffraction. The samples with different scanning strategies, i.e. hatching length, were measured in as-build condition (on a build plate) and after removal from the build plate. The absolute values of all stress components decreased after removal from the build plate. Together with surface scan utilizing a coordinate-measuring machine (CMM), it is possible to link the stress release to the sample distortion. Obtained results indicated different residual stress states for each of the transversal, longitudinal and normal component depending on the thermal gradient in the respective direction. T2 - ECNDT 2018 CY - Göteborg, Sweden DA - 11.06.2018 KW - Residual stress KW - Selective laser melting KW - Neutron diffraction KW - IN718 PY - 2018 UR - http://cdn.ecndt2018.com/wp-content/uploads/2018/05/ecndt-0315-2018-File001.pdf SP - 1 AN - OPUS4-45325 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Schaupp, Thomas A1 - Rhode, Michael A1 - Yahyaoui, Hamza A1 - Kannengießer, Thomas ED - Duprez, Lode T1 - Hydrogen distribution in multi-layer welds of steel S960QL T2 - Proceedings of the Third International Conference on Metals & Hydrogen N2 - High-strength low-alloyed (HSLA) steels with yield strength ≥ 690 MPa have increasing importance in steel construction and civil engineering. However, weld processing of those steels is a major challenge. The susceptibility for degradation of mechanical properties of weld joints significantly increases in presence of hydrogen and can result in hydrogen assisted cracking (HAC). Generally, risk for HAC increases with increasing yield strength of HSLA steels. To minimize the incidence of HAC, it is essential to gain knowledge about both the (1) absorbed hydrogen amount and its distribution in the weld seam and (2) options to lower the amount of introduced hydrogen. Existing standards recommend heat treatment procedures (interpass temperature or post weld heat treatment) to reduce the diffusible hydrogen concentration in weldments. In this context, different weld seam geometries should be considered. For HSLA steel fabrication weld processing with seam opening angles of 45° to 60° is typical. Modern weld technologies allow welding with seam opening angles of 30° - reduced welding time and costs. In the present study, the hydrogen distribution in multi-layer welds of a 960 MPa HSLA steel was analysed. Influence of different seam opening angles as well as heat input, interpass temperature and post weld heat treatments were investigated. The welded samples were quenched in ice water immediately after welding and subsequently stored in liquid nitrogen. After defined warming up, small specimens were machined from the weld seam by water jet cutting. The diffusible hydrogen concentration was measured by carrier gas hot extraction with coupled mass spectrometer. The results showed, that low heat input and post weld heat treatment procedures can lower hydrogen concentrations in welds. Furthermore, a gradient of the hydrogen concentration was identified with increasing weld pool depth. By varying the seam opening angles different hydrogen concentrations were measured. T2 - Third International Conference on Metals & Hydrogen CY - Ghent, Belgium DA - 29.05.2018 KW - Hydrogen concentration KW - Welding KW - High-strength steel KW - Heat treatment KW - carrier gas hot extraction PY - 2018 SN - 978-9-08179-422-0 SP - P44 AN - OPUS4-45358 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Griesche, Axel A1 - Pfretzschner, Beate A1 - Schaupp, Thomas A1 - Schulz, M. A1 - Kardjilov, N. ED - Duprez, Lode T1 - Hydrogen in steel visualized by neutron imaging T2 - Proceedings of the Third International Conference on Metals & Hydrogen N2 - Neutron cameras allow visualizing hydrogen distributions with radiographic or tomographic imaging methods in iron and steel. The necessary contrast between hydrogen and iron stems from the high difference in the total neutron cross section of both elements. This allows e.g. the in situ measurement of hydrogen mass flow inside cm thick steel samples with a temporal resolution of 20 s using neutron radiography as well as the quantitative measurement of hydrogen accumulations at the crack’s inner surfaces in hydrogen embrittled iron samples with neutron tomography. We could detect directly gaseous hydrogen in the crack cavities and we measured the gas pressure. This new quality of the information on a micrometer scale allows new insights for the analysis of hydrogen-induced damage mechanisms. Further, this method is non-destructive and provides local information in situ and in three dimensions with a spatial resolution of 20-30 µm. In this contribution, we show examples that demonstrate the spatial and temporal resolution of the neutron radiography and tomography methods in order to visualize and quantify hydrogen accumulations at cracks. The measurements were performed at the research reactor BER II of the HZB in Berlin and at the FRM II reactor of the neutron source Heinz Maier-Leibnitz in Garching. T2 - Third International Conference on Metals & Hydrogen CY - Ghent, Belgium DA - 29.05.2018 KW - Hydrogen KW - Steel KW - Neutron imaging PY - 2018 SN - 978-9-08179-422-0 SP - J01 AN - OPUS4-45359 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER -