TY - JOUR A1 - Rütters, H. A1 - Stadler, S. A1 - Bäßler, Ralph A1 - Bettge, Dirk A1 - Jeschke, S. A1 - Kather, A. A1 - Lempp, C. A1 - Lubenau, U. A1 - Ostertag-Hennig, C. A1 - Schmitz, S. A1 - Schütz, S. A1 - Waldmann, S. T1 - Towards an optimization of the CO2 stream composition - A whole-chain approach N2 - CO2 streams captured from power stations or industrial plants may contain impurities that impact the consecutive steps of the CO2 capture and storage (CCS) chain. As the basis for an optimization of CO2 purity over the whole CCS chain, impacts of different impurities were investigated at key steps including studies on (i) corrosion of metallic materials in CO2 streams and brine, (ii) fluid and interfacial properties as a function of pressure, temperature and CO2 stream composition and their implications for CO2 transport, injection and geological storage, (iii) costs of different pipeline design options, (iv) geochemical alterations at typical reservoir conditions and their implications for geomechanical rock properties. Major findings are synthesized for two exemplary single source-single sink CCS chain scenarios involving CO2 stream compositions typical for pre-combustion capture and oxyfuel combustion. Recommendations for material selection for compression, transport and injection were derived for various CO2 stream compositions. To reliably control corrosion, a limitation of water contents to 50 ppmv is recommended for pipeline transportation of all CO2 streams. At geological storage conditions, the presence of either O2, NOx or SO2 only weakly affected fluid-mineral/rock interactions that still impacted geomechanical rock properties. KW - CCS KW - Impurities KW - Associated incidental substances KW - Pipeline design KW - Corrosion KW - Fluid-rock interactions PY - 2016 UR - http://www.sciencedirect.com/science/article/pii/S1750583616305047 DO - https://doi.org/10.1016/j.ijggc.2016.08.019 SN - 1750-5836 SN - 1878-0148 VL - 54 IS - 2 SP - 682 EP - 701 PB - Elsevier AN - OPUS4-38401 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Pohl, K. A1 - Özcan Sandikcioglu, Özlem A1 - Voigt, M. A1 - Grundmeier, G. T1 - Adhesion and corrosive delamination of epoxy films on chemically etched ZnMgAl-alloy coatings N2 - The effect of alkaline and acidic pretreatment steps on the surface chemical composition and adhesion properties of ZnMgAl-alloy coated steel was investigated by means of spectroscopic methods, scanning Kelvin probe (SKP) and peel test measurements.The spectroscopic results indicate that the surface film composition can be adjusted by the wet-chemical treatment. To study the corresponding surface adhesive properties, the samples were coated with an epoxy amine adhesive. Peel tests under humid conditions indicated an increased interaction between the acidic pre-treated surface and the adhesive. The results of the SKP analysis show that the acidic cleaned substrates have the highest resistance to delamination, which can be explained by the shift of the interfacial electrode potential. KW - Corrosion KW - ZnMgAl-alloy coatings KW - XPS KW - Scanning Kelvin probe PY - 2016 DO - https://doi.org/10.1002/maco.201608968 SN - 0947-5117 SN - 1521-4176 VL - 67 IS - 10 SP - 1020 EP - 1026 AN - OPUS4-38196 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Bäßler, Ralph T1 - Book review: Corrosion science and technology N2 - It can be concluded, that this book fulfills its intention to be a relevant practical guide for students and professionals. The interested reader can get an insight into of all kinds of aspects one should consider when dealing with corrosion. KW - Corrosion PY - 2018 DO - https://doi.org/10.1002 maco.201870114 SN - 0947-5117 VL - 69 IS - 11 SP - 1677 EP - 1678 PB - Wiley‐VCH Verlag GmbH & Co. KGaA CY - Weinheim AN - OPUS4-46748 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Özcan Sandikcioglu, Özlem T1 - In situ imaging of corrosion processes N2 - The presentation summarizes our recent results on the coupled electrochemical methods for high resolution corrosion studies. The combination of Scanning Electrochemical Microscopy (SECM) and multielectrode (MMA) based real-time corrosion monitoring was presented as a new method for achieving high time resolution in local electrochemical analysis. Correlative imaging by means of Atomic Force Microscopy (AFM) and Scanning Electron Microscopy (SEM) was demonstrated as a tool for the investigation of local corrosion processes initiated by the intermetallic particles (IMPs) on AA2024-T3 aluminium alloy. T2 - BAM-IfW Workshop CY - Dresden, Germany DA - 28.03.2019 KW - MIC KW - Atomic Force Microscopy (AFM) KW - Corrosion monitoring KW - Corrosion PY - 2019 AN - OPUS4-50291 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Wetzel, Annica T1 - The Interplay of Anodic Passivation and Oxygen Evolution of Medium Entropy Alloys in Aqueous NaCl Electrolytes at Different pH N2 - Due to their favorable mechanical and anti-corrosion properties, medium entropy alloys (MEA) are of high academic and industrial interest as novel materials for engineering and catalytic applications. Previous studies on general corrosion behavior indicate high current densities at high anodic potentials for MEAs. Further investigations of the underlying transpassive dissolution and local corrosion behavior remain scarce. To understand the passivation behavior of MEAs CrCoNi and FeCrNi at high anodic potentials, the mechanisms of transpassive dissolution and the oxygen evolution reaction were investigated in this project. Scanning electrochemical microscopy (SECM) was applied in the interrogative mode for the detection of evolving metal species and oxygen. By means of ICP-MS analysis, dissolved metal species were quantified to provide a fundamental understanding on the transpassive dissolution. As the oxygen evolution reaction (OER) may contribute a large percentile to the observed current at high anodic potentials, SECM measurements were employed to analyze the onset of the OER. Potentiodynamic, potentiostatic and chronoamperometric techniques as well as different electrolytes were used to induce precisely controlled corrosion loads during the SECM experiments and for the ICP-MS analysis. Macroscopic corrosion properties of the alloys, electrical and chemical properties of the passive films were studied by means of potentiodynamic polarization, electrochemical impedance spectroscopy (EIS) and X-Ray Photoelectron Spectroscopy (XPS), respectively. Finally, the analysis of the corrosion morphology and the potential of the surface before, during and after passivity breakdown was carried out by means of in-situ atomic force microscopy (AFM) and scanning Kelvin probe force microscopy (SKPFM). The presentation will summarize our results on the interplay of anodic passivation and oxygen evolution of MEAs in aqueous NaCl electrolytes. T2 - MRS Spring 2023 CY - San Francisco, California, USA DA - 10.04.2023 KW - Chemically Complex Materials KW - CCMat KW - Corrosion PY - 2023 AN - OPUS4-59405 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Özcan Sandikcioglu, Özlem T1 - Changes in passive film chemistry of stainless steels in the presence of iron reducing bacteria N2 - Summary of the results obtained at DELTA-Beamline 8 in 2018. T2 - DELTA User Treffen CY - Dortmund, Germany DA - 28.11.2018 KW - MIC KW - Corrosion KW - XANES PY - 2018 AN - OPUS4-50312 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Wetzel, Annica T1 - Local corrosion properties of high/medium entropy alloys in aqueous environments N2 - High and medium entropy alloys gained increasing academic and industrial interest as novel materials for engineering applications. This project is aiming to clarify and compare the general and local corrosion properties of high entropy alloy CrMnFeCoNi and medium entropy alloy CrCoNi in different aqueous environments. The focus lies on the local corrosion processes that result either from microstructural imperfections (inclusions, defects at grain boundaries etc.) in the base material or processing related changes in the microstructure and/or local composition. The corrosion behavior of the alloys was monitored via potentiodynamic polarization experiments and the local corrosion characteristics were further investigated by means of scanning electrochemical microscopy (SECM). Their passivation behavior was analyzed in three different electrolyte systems (NaCl, H2SO4 and NaClO4; c = 0.1M). The characterization of the surface morphology and composition of the passive film was performed by means of atomic force microscopy (AFM), scanning electron microscopy coupled with energy dispersive X-Ray spectroscopy (SEM/EDX) and X-Ray photoelectron spectroscopy (XPS), respectively. Considering long term corrosion effects, electrochemical work was supported with immersion tests and the analysis of corrosion products by SEM/EDX and XPS depth-profiling. Our results indicate that the medium entropy alloy CrCoNi has a significantly higher corrosion resistance in comparison to the high entropy alloy CrMnFeCoNi. The presentation will summarize some of our results on the mechanistical aspects of the observed high corrosion resistance. T2 - EUROCORR 2020 CY - Online meeting DA - 07.09.2020 KW - High Entropy Alloys KW - Corrosion KW - Medium Entropy Alloys KW - Atomic Forc Microscopy KW - Scanning Kelvin Probe Force Microscopy KW - Potentiodynamic Polarization PY - 2020 AN - OPUS4-53787 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bäßler, Ralph T1 - A Coating System for Corrosion Protection of Carbon Steel as an Alternative for High Alloyed Materials N2 - The screening of coatings shows that the modification by adding individual pigment was not sufficient to protect carbon steel even during a short-term exposure, indicated by the discoloration after only seven days of exposure. Electrochemical tests indicated that the coating cathodically protects carbon steel or slows down the corrosion reaction. A long-term exposure test confirmed that the PANI/SiO2 modified coating successfully protects the carbon steel in the Sibayak artificial geothermal water at 150 °C for 6 months. T2 - European Geothermal Congress CY - Berlin, Germany DA - 17.10.22 KW - Corrosion KW - Geothermal KW - Coatings KW - Polyaniniline KW - Silicate PY - 2022 AN - OPUS4-56084 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Bäßler, Ralph T1 - Review: Science, Technology and Applications of Metals in Additive Manufacturing N2 - Often 3D‐printing and additive manufacturing are mentioned as the 3rd industrial revolution. In this conjunction this book provides a brief overview on additively manufactured metal pieces. This book fulfills its intension to serve as an educational guide, providing a holistic picture encompassing science, technology and applications for the real‐life use of Metal Additive Manufacturing. KW - Additive manufacturing KW - Corrosion KW - Material properties PY - 2020 DO - https://doi.org/10.1002/maco.202070114 SN - 1521-4176 SN - 0947-5117 VL - 71 IS - 11 SP - 1929 EP - 1930 PB - WILEY‐VCH Verlag GmbH & Co. KGaA CY - Weinheim AN - OPUS4-51514 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Witt, Julia T1 - Multilayer thin coatings for corrosion protection of AA2024-T3 aluminium alloy N2 - The performance of adhesively joined hybrid components relies strongly on the stability of the adhesive-material interface. With the increasing utilization of multi-material structures in the automotive and aerospace industry, it is of great scientific and technical interest to understand the processes leading to adhesive failure and to develop novel strategies to increase corrosion and delamination resistance of adhesive joints. The aim of this study is to develop thin epoxy based films and their carbon nanofiller loaded composites on aluminium alloy AA2024-T3 and to investigate their interfacial stability under corrosive and coupled corrosive-mechanical load. Spin coating was used for the layer-by-layer deposition of poly[(o-cresyl glycidyl ether)-co-formaldehyde] and poly-(ethylenimine) bi-layers. Carbon nanofillers are introduced either by mixing into the coating components or in between individual layers. Cyclic voltammetry (CV) and electrochemical impedance spectroscopy (EIS) analysis was performed to investigate the porosity and water uptake of the model films, respectively. Atomic force microscopy (AFM) results indicated a very homogeneous and dense film with low surface roughness. The bi-layer thickness ranged between 30 to 40 nm. Electrochemical measurements show a higher corrosion resistance with the increase of the bi-layer number. The main novelty of this contribution is the in-situ AFM investigations under coupled corrosive-mechanical load. For this purpose, a tensile module capable of uniaxial stretching and compression with up to 5 kN force was integrated into the AFM stage. Stretching experiments were performed to investigate the mechanical properties and adhesion of the films, as well as structural changes of the film morphology during uniaxial deformation. The contribution will provide detailed information on the new AFM setup and summarize our results on the stability of model epoxy and nanocomposite films on AA2024-T3. T2 - EURADH 2018 CY - Lisbon, Portugal DA - 05.09.2018 KW - Electrochemical Empedance Spectroscopy (EIS) KW - Scanning Kelvin Probe Force Microscopy (SKPFM) KW - Corrosion KW - Delamination KW - Aluminium KW - Epoxide PY - 2018 AN - OPUS4-46513 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bäßler, Ralph T1 - Evaluation of Corrosion Resistance of Metallic Materials in Geothermal Applications N2 - Evaluation of corrosion resistance of metallic materials is essential to assure safe and reliable operation of geothermal sites. One need to be aware that corrosion is not a material's but a system property, determined by medium, material and construction aspects. Various corrosion types have to be evaluated. Conditions in laboratory shall reflect on-site reality. Depending on brine composition and temperature suitability of metallic materials can be ranked. Most important outcome of the research is that highly saline geothermal brines require high alloyed materials, for safe long-term operation. T2 - Geothermal Essentials - Moving Geothermal Forward in Canada: Scaling and Corrosion (Surface Facilities) CY - Online Webinar DA - 16.03.2022 KW - Corrosion KW - Geothermal KW - Steel PY - 2022 AN - OPUS4-54482 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Munasir, A1 - Triwikantoro, A1 - Zainuri, M. A1 - Bäßler, Ralph A1 - Darminto, T1 - Corrosion Polarization Behavior of Al-SiO2 Composites in 1M NaCl and Related Microstructural Analysis N2 - The composites combining aluminum and silica nanoparticles with the addition of tetramethylammonium hydroxide (Al-SiO2(T)) and butanol (Al-SiO2(B)) as mixing media have been successfully fabricated. Corrosion behavior of Al-SiO2 composites before and after exposure in 1M NaCl solution was examined using potentiodynamic polarization (Tafel curve analysis). The study was also equipped with scanning electron microscopy (SEM), energy dispersive X-ray (EDX), and X-ray diffraction (XRD) investigations. Before exposure, Al-SiO2(T) exhibited the best corrosion resistance. Performance improvement was indicated by Al-SiO2(B) up to 10 times better than Al-SiO2(T) after exposure. The increased SiO2 content did not significantly enhance the corrosion resistance of the composites. The Al-SiO2 composites with 5% SiO2 content showed very high corrosion resistance (as the optimum composition). Furthermore, pitting corrosion was observed in the Al-SiO2 composites, indicated by the formation of corrosion products at grain boundaries. The product was affected by the presence of SiO2 in the Al matrix and the NaCl environment at 90 °C (approach to synthetic geothermal media: Na+, Cl, H+, OH-). Our study revealed the presence of γ-Al2O3, γ-Al(OH)3, and Al(OH)2Cl as the dominant corrosion products. KW - Al-Composite KW - Corrosion KW - Corrosion rate KW - SiO2 Nanoparticle KW - Tafel Plot PY - 2019 DO - https://doi.org/10.5829/ije.2019.32.07a.11 SN - 1025-2495 SN - 1735-9244 VL - 7 IS - 32 SP - 982 EP - 990 PB - Materials and Energy Research Center AN - OPUS4-48742 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Özcan Sandikcioglu, Özlem T1 - Combined electrochemical techniques for the investigation of corrosion processes N2 - Short presentation of BAM, a summary of the methods available in FB 6.2 and recent results on MIC and high resolution corrosion studies T2 - Institute Seminar: Jerzy Haber Institute of Catalysis and Surface Chemistry CY - Cracow, Poland DA - 07.11.2018 KW - MIC KW - Corrosion KW - Atomic Force Microscopy (AFM) KW - Combined corrosive and mechanical load PY - 2018 AN - OPUS4-50313 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bäßler, Ralph T1 - Corrosion Effects on Materials Considered for CC(U)S Applications N2 - Commercially available carbon steels are suitable for compression and pipelines as long as moisture content and impurities are limited. (water 50 to 100 ppmv, SO2 and NO2 ca. 100 ppmv) Corrosion rates increase with increasing water content. (0.2 – 20 mm/a) Condensation of acids and therefore droplet formation is always possible, even at low water contents. A low SO2 content within the CO2-stream might be more important than a low water content. Cr13-steels showed a general susceptibility to shallow pitting and pitting. So, they seem to be not suitable for CCUS applications. Low alloyed steels showed better corrosion behavior (predictable uniform corrosion). For direct contact with saline aquifer fluids only high alloyed steels shall be used. T2 - EFC Webinar CY - Online Meeting (Chongqing, China) DA - 18.05.2022 KW - Corrosion KW - CO2 quality KW - CO2 KW - CCS KW - CCU KW - Pipeline PY - 2022 AN - OPUS4-54854 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Kleinbub, Sherin T1 - The impact of methanogenic Archaea on material, environment and health N2 - Microbiologically influence corrosion (MIC) has become a big concern due the increased usage of different metals by our society. Microorganisms can use metal as an electron donor, causing unpredictable but serious damages. Nowadays it is known that besides sulfate reducing bacteria (SRB), other microorganisms including acetogens, iron oxidizers and methanogens can also induce MIC. Current studies related to methanogen-induced MIC (MI-MIC) mainly focused on environmental isolates from the oil and gas industry (e.g. Methanococcus maripaludis) with industrial materials e.g. iron. However, MI-MIC can occur in many other environments as well, including the oral cavity. Methanobrevibacter oralis is a methanogen isolated from the human oral cavity and was found more frequently in patients suffering from peri-implantitis/periodontitis. Titanium-implants removed from those patients have also showed clear signs of corrosion. The aim of our study is to establish and analyze corrosion potentials of dental metals (e.g. titanium) by oral methanogens. Periodontal pockets samples from patients suffering from periodontitis/peri-implantitis were taken for methanogenic and SRB enrichments. Stainless steel, pure titanium or Ti-6Al-4V alloy was used for corrosion studies. Corrosion rates and methane production were measured using weight-loss method and gas chromatography, respectively. Metal surfaces were visualized with scanning electron microscopy. Microbial communities in the dental pockets of healthy people and patients will be compared using 16S rRNA amplicon sequencing. Overall, this is the first study investigating the susceptibility of different dental implant materials to corrosion using human-related Archaea. The outcomes of this study can be further explored for a variety of clinical applications. T2 - ISME 17th International Symposium on Microbial Ecology CY - Leipzig, Germany DA - 12.08.2018 KW - Methanogens KW - Corrosion KW - Biofilm PY - 2018 AN - OPUS4-45932 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Koerdt, Andrea T1 - Microbial corrosion of iron coupled to methanogenesis by strains from different environments N2 - Microbially influenced corrosion (MIC) of iron is usually attributed to sulfate-reducing microorganisms (SRM) which act upon the metal by the reactiveness of hydrogen sulfide, and by withdrawal of the available electrons (Fe → Fe²⁺ + 2e⁻ ; E° = 0.47 V) in electrical contact through surface attachment. Also methanogenic archaea are supposed to cause MIC. Because they do not produce hydrogen sulfide, withdrawal of electrons may be their main corrosive mechanism; however, mechanistic details and kinetics of the overall process are poorly understood. Precipitation of siderite (4Fe + 5HCO₃⁻ + 5H⁺ → 4FeCO₃ + CH₄ + 3H₂O) can lead to an insulating layer on the metal surface and lower the corrosion rate. Still, the extent of FeCO₃ precipitation may be significantly influenced by environmental conditions such as pH and advective processes. To investigate the corrosive potential of methanogens, we studied strains isolated from marine sediments (Methanococcus maripaludis 14266, 2067, Methanobacterium-affiliated strain IM1), crude oil tanks (Methanococcus maripaludis Mic1c10, KA1) and the oral cavity (Methanobrevibacter oralis) in a closed (batch) culture, and in a sand-packed flow-through cell with pH control and simulation of a fluctuating environment. Results indicate that the rates of iron corrosion due to coupled methanogenesis (up to 0.3 mm/yr) are comparable to that caused by SRM. Surface analyses of the metal showed severe pitting. Such knowledge and deeper understanding also from an electrokinetic point of view may not only provide further models in microbial electrophysiology, but also contribute to mitigation strategies in MIC. T2 - ISME 17th International Symposium on Microbial Ecology CY - Leipzig, Germany DA - 12.08.2018 KW - Corrosion KW - Methanogens KW - Biofilm KW - Flow-System KW - Iron PY - 2018 AN - OPUS4-45735 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bäßler, Ralph T1 - Deposition of Brine Components on Materials in Geothermal Conditions T1 - ОСАЖДЕНИЕ КОМПОНЕНТОВ ГЕОТЕРМИЧЕСКИХ ВОД НА МАТЕРИАЛЫ В ГЕОТЕРМАЛЬНЫХ УСЛОВИЯХ N2 - Since geothermal wells are a feasible energy source to replace fossil fuel supply, many technologies have been developed to take advantage of geothermal energy. Nevertheless, service conditions in geothermal facilities are in many cases extreme in terms of corrosion due to the chemical composition of hydrothermal fluids and temperatures. Therefore, materials selection based on preliminary material qualification is essential to guarantee a secure and reliable operation of the facilities. During operation of a geothermal research facility in Groß Schönebeck copper and lead effects have been found downhole. Occurring mechanisms and measures to prevent precipitation or scaling needed to be investigated as well as potential influences of such precipitates on corrosion resistance of metallic materials used for equipment. This contribution deals with the evaluation of the corrosion behavior of carbon steel and corrosion resistant alloys in copper and/or lead containing artificial geothermal water, simulating the conditions in the Northern German Basin. The behavior of these materials in an artificial geothermal water obtained by electrochemical measurements and exposure tests are presented. While carbon steel exhibits precipitation and deposition, higher alloyed material shows different response to such species and a higher resistance in saline geothermal water. Basing on these results the suitability of the investigated corrosion resistant alloy is given for use in such conditions, whereas carbon steel creates difficulties due to its susceptibility to Cu- and Pb-precipitation. N2 - Поскольку геотермальные скважины являются реальным источником энергии для замены поставок ископаемого топлива, было разработано множество технологий для использования преимуществ геотермальной энергии. Тем не менее, условия эксплуатации на геотермальных установках во многих случаях являются экстремальными с точки зрения коррозии из-за химического состава гидротермальных жидкостей и температур. Таким образом, выбор материалов на основе предварительной квалификации имеет важное значение для обеспечения безопасной и надежной работы геотермальных объектов. Во время работы исследовательской установки в Грос Шёнебек (Groß Schönebeck) в скважине было обнаружено воздействие меди и свинца. Необходимо изучить возникшие механизмы и меры для предотвращения депозиции или образования коррозии, а также потенциальное влияние таких осаждений на коррозионную стойкость металлов, используемых для оборудования. Этот доклад посвящен оценке коррозионного поведения углеродистой стали и коррозионно-стойких сплавов в геотермальной воде, содержащей медь и / или свинец, моделирующей условия в Северогерманском бассейне (North German basin). Представлено поведение этих металлических материалов в геотермальной воде, полученной путем электрохимических измерений и испытаний на воздействие. В то время как углеродистая сталь демонстрирует коррозию и отложения, высоколегированный материал демонстрирует более высокую стойкость в соленой геотермальной воде. На основании этих результатов пригодность исследуемого коррозионно-стойкого сплава дана для использования в данных условиях, тогда как углеродистая сталь создает трудности из-за ее восприимчивости к депозиции солей меди и свинца. T2 - ХV International Conference Problems of Corrosion and Corrosion Protection of Materials “CORROSION-2020” CY - Online meeting DA - 15.10.2020 KW - Copper KW - Lead KW - Corrosion KW - Steel KW - Geothermal PY - 2020 UR - http://www.ipm.lviv.ua/corrosion2020/ AN - OPUS4-51438 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Aristia, Gabriela T1 - The Effect of Different Polyaniline Types in Silicon Dioxide Containing Coatings for Carbon Steel Protection in Artificial Geothermal Brines N2 - According to the results of the experiments carried out, the following points can be concluded: 1. Exposure tests showed that specimens with the addition of SiO2 particles and polyaniline particles exhibit better corrosion resistance than specimens with the addition of only polyaniline particles or binder only. 2. Open circuit potential measurements showed that in the beginning of the experiments, both coatings had an open circuit potential 100 mV higher than carbon steel. Within one day of immersion, the potential of carbon steel increased significantly, indicating the formation of oxide layer. After extended exposure the carbon steel potential sat between PS1 (which had higher potential) and PS2 (which had a lower potential) and all three were in the range –600 mV to –500 mV vs Ag/AgCl. 3. Both coatings PS-1 and PS-2 were degraded with increasing exposure time, shown by the decrease of absolute impedance value at low frequency range after 2, 4, and 6 days exposure. 4. Potentiodynamic test was performed after 3 hours and 6 days exposure, and it was shown that the coating in the initial stage exhibited more passive behavior than the specimens exposed for 6 days. T2 - NACE International Corrosion Conference 2019 CY - Nashville, TN, USA DA - 24.03.2019 KW - Geothermal KW - Coating KW - Polyaniline KW - Corrosion PY - 2019 AN - OPUS4-47914 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bäßler, Ralph T1 - Influence of brine components on materials performance in geothermal applications N2 - Significant Cu-deposition and ‑precipitation only occurred in combination with carbon steel. High-alloyed materials prevent the disturbing Cu-agglomeration. Pb-deposition and ‑precipitation only occurred in combination with carbon steel. No negative Pb-effect could be observed in combination with high-alloyed steels. High alloyed corrosion resistant alloys are suitable and shall be chosen for future design of the piping system, either in massive or in cladded form, if formation of crevices with non-metallic materials can be excluded! T2 - EUROCORR 2022 CY - Berlin, Germany DA - 28.08.2022 KW - Corrosion KW - Geothermal KW - Copper PY - 2022 AN - OPUS4-55624 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bäßler, Ralph T1 - Influence Of Brine Precipitates On Materials Performance In Geothermal Applications N2 - Significant Cu-deposition and precipitation only occurred in combination with carbon steel. High-alloyed materials prevent the disturbing Cu-agglomeration. Pb-deposition and precipitation only occurred in combination with carbon steel. No negative Pb-effect could be observed in combination with high-alloyed steels. High alloyed corrosion resistant alloys are suitable and shall be chosen for future design of the piping system, either in massive or in cladded form, to prevent unwanted interactions with brine components. T2 - AMPP Annual 2023 Conference CY - Denver, CO, USA DA - 19.03.2023 KW - Geothermal KW - Electrochemistry KW - Copper KW - Lead KW - Corrosion PY - 2023 AN - OPUS4-57237 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bäßler, Ralph T1 - Integrated Coating System for Corrosion Protection of Carbon Steel in Artificial Geothermal Brine N2 - Corrosive geothermal brines are a major challenge to geothermal power-plants. For cost reasons, plant designers prefer to use carbon and low alloyed steels, which are susceptible to uniform and localized corrosion when exposed to geothermal brines having acidic and saline properties. To solve such problem, coatings or inhibitors would be a protective solution as an alternative to the use of high alloyed materials. This study investigated a coating system consisting of polyaniline/silicon dioxide based on resources locally available in Indonesia. Protection against corrosion of carbon steel was shown by long-term (28 day) exposure and electrochemical tests of coated carbon steels, performed in an artificial acidic and saline geothermal brine, comparable to the conditions encountered at a site in Indonesia. Therefore, an integrated coating system is proposed for corrosion protection, combining the electrochemical functionality of polyaniline and the physical advantages of silica. T2 - AMPP International Corrosion Conference 2022 CY - San Antonio, TX, USA DA - 08.03.2022 KW - Geothermal KW - Corrosion KW - Coating KW - Polyaniline KW - Silicon dioxide PY - 2022 AN - OPUS4-54452 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bäßler, Ralph T1 - Challenges for corrosion resistance of metallic materials in geothermal applications N2 - Corrosion aspects for use of metallic materials in geothermal applications are presented and discussed. T2 - Corrosion Workshop beim Geothermie Kongress 2018 CY - Essen, Germany DA - 27.11.2018 KW - Corrosion KW - Geothermal KW - Steel PY - 2018 AN - OPUS4-46744 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Merino, E. A1 - Cere, S. A1 - Özcan Sandikcioglu, Özlem A1 - Dimper, Matthias A1 - Sobrados, I. A1 - Durán, A. A1 - Castro, Y. T1 - Influence of the BF3·O(C2H5)2 on the corrosion resistance of hybrid silica sol-gel coatings deposited on flash-PEO-treated Mg alloy N2 - Achieving highly cross-linked sol-gel coatings to provide effective corrosion protection of Mg alloys remains a challenging task. The aim of this work is to evaluate the effect boron trifluoride diethyl etherate (BF3·O(C2H5)2) as catalyst to epoxy group in a GPTMS/TEOS/SiO2 sol and assesses its effect on the structure and corrosion resistance properties of Flash-PEO coated pre-treated Mg alloy. 29Si MAS NMR and 13C CPMAS-NMR demonstrated that (BF3·O(C2H5)2) efficiently promotes the epoxy polymerization of the GPTMS and the formation of a hybrid silica network. However, the amount of (BF3·O(C2H5)2) should be optimized to minimize the formation of undesirable byproducts such as ethyl ether terminal units. Therefore, GPTMS/TEOS/SiO2 sols containing different amounts of (BF3·O(C2H5)2) were synthesized and deposited onto the Flash-PEO coated Mg alloy, leading to bilayer systems with a total thickness of ⁓8 μm. The corrosion behavior of the bilayer coatings in 3.5 wt% NaCl solution was evaluated by electrochemical impedance spectroscopy (EIS) and Scanning Kelvin probe microscope (SKPFM). The results revealed that the barrier properties of the coatings with enhanced cross-linked structure showed impedance modulus (│Z│f:0.1 Hz) approximately four orders of magnitude higher than the bare magnesium alloy and two orders of magnitude higher than the F-PEO coated sample. A suitable compromise between (BF3·O(C2H5)2) amount and sol-gel film structure is required to obtain a more durable barrier coating capable to extend the protective lifespan of the magnesium alloy. KW - Sol-gel KW - Corrosion KW - AZ31B Mg alloy KW - Chemical structure KW - SKPFM PY - 2026 DO - https://doi.org/10.1016/j.surfcoat.2025.133055 SN - 0257-8972 VL - 522 SP - 1 EP - 13 PB - Elsevier B.V. AN - OPUS4-65416 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Özcan Sandikcioglu, Özlem T1 - Exploration of Fe-Ni-Cr-X systems using diffusion couples for new alloy chemistries with improved mechanical and corrosion properties N2 - Multi-principal element alloys (MPEAs) are disrupting methodologies in conventional alloy design, characterized by a singular dominant element dictating composition. The traditional optimization of the functional properties of alloys primarily relies on microalloying techniques. The advent of MPEAs has significantly broadened the chemical landscape available for exploration, approaching near-infinite possibilities. Consequently, innovative methodologies are imperative for discovering new alloys that exhibit properties customized for specific applications, simultaneously mitigating dependence on critical minerals. One promising approach for rapid screening of possible alloy chemistries and exploring the hitherto untouched regions of ternary, quaternary or higher order phase diagrams is the use of diffusion couples and multiples. The present study focusses on the exploration of quaternary multi-principle-element alloys (MPEAs) using diffusion multiples. We established diffusion systems by combining an equimolar ternary alloy (FeNiCr) with single diffusing elements Mn, Mo and Ta. Using ThermoCalc® and DICTRA® simulations, we determined suitable parameters (temperature and diffusion time) that would lead to the formation of single-phase alloys and diffusion lengths (>50 μm) that suit the application of high-resolution characterization methods. Microstructural and compositional characterization was performed via scanning electron microscopy (SEM) and energy dispersive X-ray spectroscopy (EDX), electron probe microanalyzer (EPMA) and correlated to local mechanical properties evaluated by means of nanoindentation. Selected compositions from the diffusion couples were recast and homogenized to obtain bulk samples for the assessment of high-temperature and aqueous corrosion properties. Our results indicate that the ThermoCalc simulations have a good predictive power for crystallographic phases for Mn and Mo containing MPEAs derived from the diffusion couples. Moreover, our data on FeCrNi-Ta system provides valuable experimental input for respective databases necessary for simulation of phase diagrams. The presentation will summarize our methodology using diffusion couples as an efficient tool for exploring compositional spaces of MPEAs in the search for novel alloy chemistries and the results of our correlative study on the mechanical and corrosion properties of the selected quaternary systems. T2 - EUROCORR 2024 CY - Paris, France DA - 01.09.2024 KW - CCMat KW - Corrosion KW - Diffusion couples KW - Multi-principal element alloys PY - 2024 AN - OPUS4-62634 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Özcan Sandikcioglu, Özlem T1 - Untersuchung lokaler Korrosionsprozesse mittels kombinierter elektrochemischer und mikroskopischer Methoden N2 - Aktuelle Forschungsergebnisse - Korrosionseigenschaften von AA 2024-T3 und AM-316 unter gekoppelter korrosiv/mechanischer Beanspruchung. T2 - MPIE Düsseldorf, Sitzung der GfKORR Arbeitskreise Grundlagen und Simulation und Korrosionsuntersuchung und überwachung CY - Dusseldorf, Germany DA - 20.11.2019 KW - Corrosion KW - Atomic Force Microscopy (AFM) KW - Coupled corrosive/mechanical load PY - 2019 AN - OPUS4-50296 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Aristia, Gabriela T1 - SiO2-containing organic coatings for geothermal application N2 - Geothermal brine is considered to be an aggressive environment as it contains various dissolved salts. Even though carbon steel is commonly used as a construction material due to its machinability and economical reason, it is susceptible to uniform and localized corrosion in a high temperature and high pressure system. Therefore, a coating system is introduced to protect the carbon steel against corrosion in such environment. -It is necessary to find the optimum composition of SiO2 addition in the organic coatings to enhance the material performance, i.e. coatings adhesion, thickness optimization, thermal resistance. Current project aims at the addition of Polyaniline (PANi) as the active agent to improve the corrosion resistance of materials against a high saline medium at elevated temperatures. T2 - BAM PhD Day CY - Berlin, Germany DA - 21.09.2017 KW - Geothermal KW - Corrosion KW - Coating PY - 2017 AN - OPUS4-43362 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Koerdt, Andrea T1 - Methanogenic Archaea N2 - Different environmental samples reveal that methanogenic Archaea are part of a multi-species biofilm on corroding metallic structures. Studies on microbial influenced corrosion (MIC) focus mainly on sulphate reducing Bacteria (SRB), leading to the assumption that they are exclusively responsible for metal corrosion. In fact, methanogenic Archaea are known to be involved in metal corrosion as well (e.g. Methanococcus maripaludis DSM 2067). In some cases SRB and methanogenic Archaea have comparable high corrosion rates. However, the underlying mechanisms causing corrosion are still unknown. The goal of this study is to develop suitable methods for analyzing two environmental isolates (M. maripaludis DSM 2067, M. maripaludis KA1) and two human-related isolates (Methanobrevibacter oralis and Methanobrevibacter smithii) for their ability to deteriorate/transform metals, which are relevant for technical and clinical applications. Moreover, the studies will provide essential information on the interaction mechanisms of human-related Archaea, which are frequently found in peri-implantitis, with dental material such as implants, crowns and bridges leading to their degradation and transformation. T2 - DECHEMA-GfKORR-Fachgruppe CY - Berlin, Germany DA - 04.10.2017 KW - Biofilm KW - Corrosion KW - Methanogens PY - 2017 AN - OPUS4-43025 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Wurzler, Nina T1 - Effect of adsorbed organic thin films on electrochemical interaction mechanisms of metal reducing bacteria with steel surfaces N2 - The interface of a metal substrate and a biofilm can differ significantly from the surrounding environment. Metal reducing bacteria (MRB), for instance, are capable of utilizing various metallic compounds as electron acceptors. Besides chromium, uranium and manganese as well as many organic compounds, Fe(III) is converted to the soluble form Fe(II) during the bacterial metabolism. This could lead to a weakening of the protective passivation layer on stainless steel and thereby facilitate microbiologically influenced corrosion (MIC). Even tough the processes of electron transfer are not yet entirely explained, the contribution of flavins and other humic substances as electron shuttles is widely discussed in the literature. Moreover, the adsorption of organic thin films on steel surfaces can lead to surface preconditioning and thus to changes in adhesion behavior of bacteria. The aim of this work is to understand the chemical and electrochemical interaction mechanisms of MRB with steel surfaces by combining electrochemistry and surface-analytical techniques. The investigations primarily focus on the effect of pre-adsorbed thin organic films and self-assembled monolayers (SAMs) on the electron transfer processes between bacteria and steel surfaces. Electrochemical Quartz Crystal Microbalance (eQCM) studies have been performed to investigate the adsorption/desorption kinetics of organic films as well as the formation of biofilms on FeCr electrodes. Furthermore, the evolution of the biofilms on steel surfaces has been analyzed by means of electrochemical impedance spectroscopy (EIS) to support the QCM studies with information on structural changes during different stages of biofilm growth. Electron transfer and corrosion processes have been analyzed by means of square wave voltammetry (SWV) and linear sweep voltammetry (LSV), respectively. The results of electrochemical studies are complemented with microscopic and spectroscopic characterisation of organic adsorbates and analysis of changes in the passive film chemistry and surface morphology. This presentation will summarize our results on the chemical and electrochemical interaction mechanisms of MRB on steel surfaces leading to passive film degradation. The role of flavins in accelerating corrosion processes will be elucidated in detail to provide useful insights from a fundamental aspect for the understanding of the initial stages of microbiologically influenced corrosion in the presence of MRB. T2 - 232nd ECS Meeting CY - National Harbor, MD, USA DA - 01.10.2017 KW - Flavins KW - Metal reducing bacteria (MRB) KW - Microbiologically influenced corrosion (MIC) KW - Corrosion PY - 2017 AN - OPUS4-43463 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Dimper, Matthias A1 - Hampel, Marco T1 - Multielectrode array probes for early detection of corrosion processes N2 - Multielectrodes are arrays of single electrodes arranged in a particular geometry. In our work, all the single electrodes are identical stainless steel X5CrNi18-10 (1.4301) wire electrodes. Using a multielectrode analyser all single electrodes are connected via zero resistance ammeters, simulating a galvanically coupled single electrode surface. The advantage of the multielectrode analyser (MMA) is that the currents flowing between single electrodes can be measured. Thus, real-time maps can be generated indicating where anodic and cathodic areas lie on the surface of the multielectrode and how they behave. The combination of the multielectrode analyser with the scanning electrochemical microscopy (SECM) enables the identification of corrosion sites and the detailed electrochemical analysis. T2 - DECHEMA/GfKORR-Fachgruppe "Mikrobielle Materialzerstörung und Materialschutz" CY - Berlin, Germany DA - 04.10.2017 KW - Scanning electrochemical microscope (SECM) KW - Multielectrode array sensors KW - Corrosion PY - 2017 AN - OPUS4-43461 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Hampel, Marco T1 - A new approach for high-resolution analysis of early-stage corrosion processes N2 - The poster presentation summarizes the recent developments on the combination of scanning electrochemical microscopy with multielectrode arrays for the investigation of local corrosion processes. T2 - GfKORR Jahrestagung 2017 CY - Frankfurt am Main, Germany DA - 07.11.2017 KW - Scanning electrochemical microscope (SECM) KW - Multielectrode array sensors KW - Corrosion PY - 2017 AN - OPUS4-43459 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Bäßler, Ralph T1 - Book review: Corrosion control through organic coatings N2 - Finally it can be summarized that this book fulfills its intention of providing theoretical background and examples for practical applications of coatings used for corrosion protection. It can be recommended to those being interested in coatings, serving as an overview on aspects which needs to be considered when working with such systems. KW - Coating KW - Corrosion KW - Pipeline PY - 2017 DO - https://doi.org/10.1002/maco.201770094 SN - 1521-4176 VL - 68 IS - 9 SP - 1014 EP - 1014 PB - WILEY-VCH Verlag GmbH & Co. KgaA CY - Weinheim AN - OPUS4-43706 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Bäßler, Ralph T1 - Book review: Challenges in corrosion N2 - Finally it can be concluded that this book fulfills its aim of being an attempt to present the subject of corrosion in a simple form. It introduces students into the world of corrosion making them familiar with general knowledge and certain kinds of approaches of assessing corrosion. KW - Corrosion KW - Material KW - Cost PY - 2017 DO - https://doi.org/10.1002/maco.201770044 SN - 1521-4176 VL - 68 IS - 4 SP - 484 EP - 484 PB - WILEY-VCH Verlag GmbH & Co. KgaA CY - Weinheim AN - OPUS4-43697 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Aristia, Gabriela T1 - Polyaniline/silicon dioxide containing coating for use in artificial geothermal brines N2 - Geothermal brine is a complex system containing a wide variety of dissolved salts resulting from the condition s in a geothermal well. These fluids lead to corrosion in pipes and other parts of geothermal system construction and necessitate intense research efforts in finding new suitable materials. Carbon steel is susceptible to corrosion in geothermal brine especially when it is exposed to a high temperature and high-pressure medium, which is considered to be an aggressive environment. An artificial geothermal water, bas ed on a brine composition found in Indonesia, was used to investigate the performance of high alloyed materials. The electrolyte has pH 4 and contains 1,500 mg/l Cl-, 20 mg/l SO4 2-, 15 mg/l HCO3 -, 200 mg/l Ca 2+, 250 mg/l K+, and 600 mg/l Na+. In order to protect the bare material in geothermal application, it is necessary to either use high alloyed material s or coatings. In this research, a coating system consisting of polyaniline and silicon dioxide was investigated regarding its behavior to protect carbon steel. In detail, the effect of SiO2 and polyaniline (PANi) addition was evaluated by exposure and electrochemical tests for 7 days, i.e. electrochemical impedance spectroscopy (EIS) and open circuit potential (OCP) at room temperature and 150 °C with 1 MPa pressure. T2 - NACE International Annual Corrosion Conference CY - Phoenix, AZ, USA DA - 15.04.2018 KW - Geothermal KW - Coating KW - SiO2 KW - Polyaniline KW - Corrosion PY - 2018 AN - OPUS4-44919 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Aristia, Gabriela T1 - Electrochemical study of polyaniline/silicon dioxide containing coatings in geothermal solution N2 - Polyaniline/Silicon Dioxide containing coatings were electrochemically investigated in a saline geothermal solution. With the increase of exposure time, impedance values of coated specimens decreased at low frequency, which could be caused by the decrease of pore resistance due to electrolyte or water uptake. Coating system needs further optimization work. T2 - NACE International Annual Corrosion Conference CY - Phoenix, AZ, USA DA - 15.04.2018 KW - Geothermal KW - Coating KW - SiO2 KW - Polyaniline KW - Corrosion PY - 2018 AN - OPUS4-44918 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Schenderlein, Matthias T1 - Monitoring early stage corrosion processes during biofilm formation N2 - To investigate early stage corrosion processes of stainless steel 1.4301 taking place during the biofilm formation of the organism Shewanella putrefaciens electrochemical impedance spectroscopy (EIS) in a multielectrode approach has been used. The multielectrode array consisted of up to 25 electrically isolated electrodes made of stainless steel wires of diameters ranging from 100 µm to 500 µm. They were connected to a multichannel microelectrode analyzer (MMA) electrically coupled through zero resistance ammeters. Current flow between electrodes in the array as well as changes in impedance of individual electrodes over time were recorded and analyzed with respect to the onset of localized corrosion and biofilm formation. The results were complemented by optical microscopy, SEM and AFM images which were taken immediately after the respective experiment. To verify that the multielectrode arrays correctly indicated the initial stages of the corrosion process and of biofilm formation they were introduced in a flow cell reaction vessel containing test specimens made from stainless steel 1.4301, which were checked regularly for signs of localized corrosion and biofilms. Preceding results with the multielectrode array in solutions containing high amounts of chloride ions and hydrogen peroxide at low pH also showed that it is possible with the MMA to monitor individual electrodes becoming local anodes as local corrosion set in, while the remaining electrodes predominantly acted as cathodes. T2 - 69th Annual Meeting of the International Society of Electrochemistry CY - Bologna, Italy DA - 02.09.2018 KW - Corrosion KW - Multielectrode KW - Biofilm KW - Monitoring KW - Stainless steel PY - 2018 AN - OPUS4-47095 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Bäßler, Ralph T1 - Review: Corrosion Atlas Case Studies - 2019 Edition N2 - This edition, published as first issue within the series “Corrosion Atlas”, provides 181 corrosion case studies, collected from 29 contributors. These Corrosion Atlas Case Studies provide a helpful tool required for engineers in their daily life to quickly determine and solve their equipment's corrosion problems by compact theoretical background and vivid examples. It fulfills the intension of the editors to be “the first centralized collection of case studies containing challenges paired directly with solutions together in one location”. KW - Corrosion KW - Failure KW - Water-bearing PY - 2020 DO - https://doi.org/10.1002/maco.202070054 SN - 1521-4176 SN - 0947-5117 VL - 71 IS - 5 SP - 859 PB - WILEY‐VCH Verlag GmbH & Co. KGaA CY - Weinheim AN - OPUS4-50757 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Valet, Svenja A1 - Bohlmann, Tatjana A1 - Ebell, Gino A1 - Burkert, Andreas T1 - pH sensitive gel pads for the visualization of anodes and cathodes on zinc N2 - Zinc and zinc alloys have many applications. Zinc corrosion takes place in the atmosphere and is assumed to follow the water drop theory (a macroelement), in which the anode is at the centre of the drop and is surrounded by a cathode. This paper is the first to use gel electrolytes made of agar to visualize anodic and cathodic areas on zinc samples in order to examine the water drop theory. For that, agar gels were added with universal pH indicators, as the anode and cathode exhibit different pH values. In this paper, different amounts of pH indicators were tested to determine whether the indicator influences the potential, the impedance, phase shift, corrosion current and potential and corrosion layer resistance. KW - Corrosion KW - Zinc KW - Gel electrolyte PY - 2026 DO - https://doi.org/10.1016/j.electacta.2026.148134 SN - 0013-4686 VL - 551 SP - 1 EP - 21 PB - Elsevier Ltd. AN - OPUS4-65308 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Armatys, Kamila A1 - Adamczyk, Burkart A1 - Adam, Christian A1 - Pflumm, R. A1 - Galetz, M. C. T1 - Corrosion and abrasion resistant protective coatings for biomass combustion N2 - The environmental concerns about availability of fossil fuels and greenhouse gas effect increase and alternative renewable fuels for power plants are gaining significantly of importance. One of the alternative renewable fuels is biomass but it is a difficult fuel because of its diversity and complexity. It can contain high percentages of K and Cl responsible for corrosion together with sand that have additionally an abrasive effect during combustion. Because of permanently extending the surface reaction due to abrasion the corrosion of the materials increases. In particular in power plants, the superheater tubes are exposed to a corrosive abrasive attack that is one of the main sources of concern. The development of new alloys for multilayer surface, which combines corrosive and abrasive resistance is therefore of high importance. Those new technical approaches must be at the same time cost-effective to be an alternative to conventional materials. This paper presents the principle of experimental methods developed for the investigations of high temperature corrosion combined with abrasion in thermochemical processes with high hydrochloric acid concentrations like during biomass combustion. The aim of the presented investigation methods it to test and develop suitable alloys for coatings for the super heater tubes of biomass power plants. First results of abrasion investigations show improved abrasion resistance compared to the multi-component reference material Alloy 625. T2 - Young Researchers Conference: Energy Efficiency & Biomass CY - Wels, Austria DA - 24.02.2016 KW - Corrosion KW - Coatings PY - 2016 SP - 1 EP - 9 CY - Proceedings in Young Researchers Conference: Energy Efficiency & Biomass 2016 AN - OPUS4-35714 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Armatys, Kamila T1 - Corrosion and abrasion resistant protective coatings for biomass combustion N2 - One of the alternative renewable fuels is biomass but it is a difficult fuel because of its diversity and complexity. It can contain high percentages of K and Cl responsible for corrosion together with sand that have additionally an abrasive effect during combustion. Because of permanently extending the surface reaction due to abrasion the corrosion of the materials increases. In particular in power plants, the superheater tubes are exposed to a corrosive abrasive attack that is one of the main sources of concern. The development of new alloys for multilayer surface, which combines corrosive and abrasive resistance is therefore of high importance. Those new technical approaches must be at the same time cost-effective to be an alternative to conventional materials. The aim of the presented investigation methods is to test and develop suitable alloys for coatings for the super heater tubes of biomass power plants. First results of abrasion investigations show improved abrasion resistance compared to the multi-component reference material Alloy 625. T2 - Young Researchers Conference: Energy Efficiency & Biomass CY - Wels, Austria DA - 24.02.2016 KW - Coatings KW - Corrosion PY - 2016 AN - OPUS4-35713 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Breitenbach, Romy A1 - Silbernagl, Dorothee A1 - Toepel, J. A1 - Sturm, Heinz A1 - Broughton, William J. A1 - Sassaki, G. L. A1 - Gorbushina, Anna T1 - Corrosive extracellular polysaccharides of the rock-inhabiting model fungus Knufia petricola N2 - Melanised cell walls and extracellular polymeric matrices protect rock-inhabiting microcolonial fungi from hostile environmental conditions. How extracellular polymeric substances (EPS) perform this protective role was investigated by following development of the model microcolonial black fungus Knufia petricola A95 grown as a sub-aerial biofilm. Extracellular substances were extracted with NaOH/formaldehyde and the structures of two excreted polymers studied by methylation as well as NMR analyses. The main polysaccharide (~ 80%) was pullulan, also known as α-1,4-; α-1,6-glucan, with different degrees of polymerisation. Αlpha-(1,4)-linked-Glcp and α-(1,6)-linked-Glcp were present in the molar ratios of 2:1. A branched galactofuromannan with an α-(1,2)-linked Manp main chain and a β-(1,6)-linked Galf side chain formed a minor fraction (~ 20%). To further understand the roles of EPS in the weathering of minerals and rocks, viscosity along with corrosive properties were studied using atomic force microscopy (AFM). The kinetic viscosity of extracellular K. petricola A95 polysaccharides (≈ 0.97 × 10-6 m2 s-1) ranged from the equivalent of 2% (w/v) to 5% glycerine, and could thus profoundly affect diffusion-dominated processes. The corrosive nature of rock-inhabiting fungal EPS was also demonstrated by its effects on the aluminium coating of the AFM cantilever and the silicon layer below. KW - Corrosion KW - EPS KW - Melanised microcolonial fungi (MCF) KW - Pullulan KW - Sub-aerial biofilms (SAB) KW - α-1,4- and α-1,6-glucans KW - AFM cantilever vibration KW - Nanoviscosity KW - Nanocorrosion of aluminium and silicon PY - 2017 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-435910 DO - https://doi.org/10.1007/s00792-017-0984-5 SN - 1433-4909 SN - 1431-0651 VL - 22 IS - 2 SP - 165 EP - 175 PB - Springer CY - Berlin AN - OPUS4-43591 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bäßler, Ralph T1 - Corrosion stability of piping steels in a circulating supercritical impure CO2 environment N2 - In supercritical impure CO2 (worst case scenario) highly alloyed Steels tend to pitting corrosion; iron and carbon steel tend to General corrosion, however, with low corrosion rates (< 0.1 mm/a) T2 - Kolloquium Uni Potsdam CY - Potsdam, Germany DA - 18.3.2016 KW - CCS KW - CO2 KW - Corrosion PY - 2016 AN - OPUS4-36990 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bäßler, Ralph T1 - Pinguin di Jerman: Apa hubungannya dengan korosi? T1 - Penguins in Germany: What does it has to do with corrosion? N2 - A failure case in an animal enclosure at Hannover Zoo is presented. Reasons for corrosive failure and solutions are discussed. T2 - Lecture at Institut Teknologi Sepuluh Nopember (ITS) CY - Surabaya, Indonesia DA - 12.11.2018 KW - Corrosion KW - Marine PY - 2018 AN - OPUS4-46741 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Koerdt, Andrea T1 - Microbial corrosion of iron coupled to methanogenesis by strains from different environments N2 - Microbially influenced corrosion (MIC) of iron is usually attributed to sulfate-reducing microorganisms (SRM) which act upon the metal by the reactiveness of hydrogen sulfide, and by withdrawal of the available electrons in electrical contact with the metal. Methanogenic archaea are supposed to cause MIC. Because they do not produce hydrogen sulfide, withdrawal of electrons may be their main corrosive mechanism; however, mechanistic details and kinetics of the overall process are poorly understood. Precipitation of siderite (4Fe + 5HCO3 + 5H+  4FeCO3 + CH4 + 3H2O) can lead to an insulating layer on the metal surface and lower the corrosion rate. Still, the extent of FeCO3 precipitation may be significantly influenced by environmental conditions such as pH and advective processes. T2 - ISME CY - Leipzig, Germany DA - 12.08.2018 KW - Methanogens KW - MIC KW - Corrosion KW - Environmental Simulation PY - 2018 AN - OPUS4-46397 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Beck, Joana T1 - Book review: Handbook of material weathering (6th edition) N2 - With its almost 1000 pages and 1.7 kg this handbook feels like holding the holy bible for users of weathering techniques as well as for technicians, engineers and scientist planning to test polymeric products behavior in natural or artificial environments. KW - Corrosion KW - Testing PY - 2019 DO - https://doi.org/10.1002/maco.201970014 SN - 0947-5117 VL - 70 IS - 1 SP - 170 EP - 171 PB - Wiley-VCH CY - Weinheim AN - OPUS4-47149 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Seneschal-Merz, Karine A1 - Bücker, Michael A1 - Feldmann, Ines T1 - Low melting glasses for transparent and environmentally-resistant enamels N2 - Today glass is broadly used in modern architecture. For indoor applications it is possible to produce decorated glass by using enamel colours and glass painting techniques without any problems. However, this is more limited for applications out of doors. Humidity and environmental pollution attack the surface of the coating and can damage it. There are only a few colours on the market which are resistant towards acids and bases until now. Additionally, most of those colours are opaque. To extend the colour palette, chemically resistant low melting coloured glasses are being developed which are transparent and intensively toned even in thin coating thicknesses. To achieve such an ambitious aim, many parameters have to combine and act in a complex manner. New compositions of lead borosilicate, zinc borosilicate and lead-zinc borosilicate glasses were produced and milled as powder. The thermal properties as well as the environmental stability were analysed. The influence of PbO and ZnO on the thermal properties and the environmental stability were investigated. Evaluation of the fusing results shows that the production and mixture of transparent vitreous enamels for the exterior side of glasses is possible. The tests made it clear that the original materials for making the vitreous enamels must be excellently ground and prepared to achieve a satisfactory result. The method to produce durable vitreous enamels for exterior application also seems to allow the production of glass colours. KW - Low melting glasses KW - Enamels KW - Heavy metal free KW - Corrosion KW - Chemical durability KW - Aging tests KW - Architecture KW - Colored glasses PY - 2019 DO - https://doi.org/10.13036/17533546.60.4.002 SN - 1753-3546 SN - 1753-3554 VL - 60 IS - 4 SP - 97 EP - 104 PB - Society of Glass Technology CY - Sheffield, UK AN - OPUS4-48835 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bäßler, Ralph A1 - Stoljarova, A. A1 - Regenspurg, S. T1 - Material qualification in Saline, copper containing geothermal water N2 - By exposure and electrochemical tests in the laboratory the Cu-effect on corrosion behavior of carbon steel, high-alloyed steels and Ti-alloy can be assessed. Critical materials specific properties were determined by static exposure and electrochemical tests in an artificial geothermal water with high salinity and low pH, containing Cu. Conclusions were drawn using characteristic potential values. It could be shown that significant Cu-deposition and -precipitation only occurred in combination with carbon steel. High-alloyed materials (S31603, S31653, S31700, S31703, S31803 and N08904) prevent the disturbing Cu-agglomeration. Therefore, they are suitable to be chosen for future design of the piping system, either in massive or in cladded form, if formation of crevices with non-metallic materials can be excluded. From the interactions and pitting corrosion point of view, R50400 seems to be most favorable. T2 - NACE International Corrosion Conference 2019 CY - Nashville, TN, USA DA - 24.03.2019 KW - Copper KW - Corrosion KW - Steel KW - Geothermal energy PY - 2019 SP - 1 EP - 11 PB - NACE International CY - Houston AN - OPUS4-47911 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Aristia, Gabriela A1 - Nofz, Marianne A1 - Bäßler, Ralph A1 - Sojref, Regine A1 - Le, Quynh Hoa T1 - Preliminary Study on Al2O3 Sol-Gel Coating for Corrosion Protection of Martensitic Stainless Steel in Artificial Geothermal Water N2 - Al2O3 coatings are often used as protective layers on steels against electrochemical and high-temperature corrosion because they are chemically inert and stable at elevated temperatures. This study presents preliminary work on the possibilities of using Al2O3 sol-gel coatings for corrosion protection of martensitic stainless steels in geothermal environments. Al2O3 sol-gel coatings were applied on UNS S42000, which is known to be susceptible to uniform and localized corrosion. The coated steel specimens were then tested in two types of artificial geothermal water, which simulate the geothermal fluids found in Sibayak (SBY), Indonesia, and North German Basin (NGB), Germany, respectively. SBY has pH 4 and 1.5 g/L of chloride ions, whereas NGB has a pH of 6 and 166 g/L of chloride ions. All experiments were carried out in autoclaves at 150 °C and 1 MPa under the deaerated condition. Evaluations were performed by investigating the surface profiles of both uncoated and coated steels before and after the corrosion test using a Laser Scanning Microscope (LSM) and Scanning Electron Microscope (SEM). Finally, Electrochemical Impedance Spectroscopy (EIS) was performed to compare the corrosion resistance of Al2O3 coated steels in SBY and NGB solutions. It was observed from the corrosion test that Al2O3 coatings are more suitable for use in the geothermal water with a higher pH. T2 - AMPP Annual International Corrosion Conference 2021 CY - Online Meeting DA - 19.04.2021 KW - Protective coating KW - Sol-gel coating KW - Geothermal KW - Martensitic steel KW - Corrosion PY - 2021 SP - 16777-01 EP - 16777-12 CY - Houston AN - OPUS4-52501 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Witt, Julia T1 - In situ AFM studies of deformation and corrosion processes on AA2024-T3 aluminium alloy N2 - The performance of functional coatings and adhesively joined hybrid components relies strongly on the stability of the polymer-metal interface. With the increasing utilization of multi-material structures in the automotive and aerospace industry, it is of great scientific and technical interest to understand the processes leading to interface degradation and to develop novel strategies to increase corrosion and delamination resistance. The aim of this project is to develop thin epoxy-based films on aluminium alloy AA2024-T3 as a model system and to investigate their interfacial stability under corrosive and coupled corrosive-mechanical load. Electrochemical and spectroscopic methods were used for the characterisation of the film properties and in situ corrosion experiments were performed by means of AFM. The deformation properties of the aluminium alloy and the model coatings were investigated by means of scanning Kelvin probe force microscopy (SKPFM) utilizing the integrated tensile stage. The presentation will give a brief overview of the capabilities of the new AFM setup to foster future collaborations and summarize our work on the interface stability of model coatings. T2 - Abteilungskolloquium FB6 CY - Berlin, Germany DA - 27.11.2018 KW - Corrosion KW - In situ Atomic Force Microscopy (AFM) KW - Aluminium alloy KW - Scanning Kelvin Probe Force Microscopy (SKPFM) PY - 2018 AN - OPUS4-48027 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bäßler, Ralph T1 - Compatibility of polymers exposed to heating oil blends with 10 % and 20 % biodiesel (FAME) N2 - Biodiesel (FAME) from rapeseed is an environmentally friendly alternative to common fossil fuels. It is also suitable to serve as blending component to fuels like heating oil. If the fuel composition is changed, materials compatibility must be guaranteed. Adding polar biodiesel to nonpolar heating oil, changes the blend’s solvency and might cause swelling, extraction and solvation of polymers. The objective of this research was to investigate the compatibility of polymeric materials, which are commonly used for components in middle distillate facilities, along with blends of heating oil and 20 % biodiesel (B20). For this propose, ACM, HNBR, FKM, PE, PA 6, POM, PUR and PVC were exposed to heating oil and B20 for 42 and 84 days at 40 °C. In addition, the polymers HNBR, FKM, PA, POM and PVC were also exposed at 70 °C. Furthermore, the resistance of polymers in eight-year aged B10 at 40 °C was evaluated. Ageing of biodiesel increases acidity which might propagate polymer corrosion. The materials were evaluated as resistant, if the loss in tensile properties (tensile strength and elongation at break) and Shore hardness remained under 15 % compared to the initial unexposed material values. For investigations under compressed conditions, the compression set was determined for specimens of ACM, FKM and HNBR after exposure in heating oil B0 and B20 for 3,7,14, 28, 56 and 90 days at 40 °C according to ISO 815-1. It was found that the resistance in B20 at 40 °C was given for all tested polymers except PUR. In the 8 years aged B10, PUR and POM were not compatible and ACM just conditionally compatible. At 70 °C, FKM and PVC were resistant in B20, whereas HNBR and PA 6 were not compatible. Swelling occurred for the elastomers ACM, HNBR and PUR. T2 - AMPP Annual International Corrosion Conference CY - Online Meeting DA - 19.04.2021 KW - Biodiesel KW - FAME KW - RME KW - Polymer in fuels KW - Corrosion PY - 2021 AN - OPUS4-52498 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bäßler, Ralph T1 - On the corrosion mechanism of CO2 transport pipeline steels caused by impurities: Roles of each impure components and benchmarks N2 - Carbon Capture, Utilization and Storage (CCUS) has been proposed as a promising technology for the mitigation of CO2 emissions into the atmosphere from fossil-fuel- operated power generation plants. As the reliability and cost effectiveness of the Pipeline transport network is crucial to the Overall operability and resilience of the CCUS system, it is vital to realize the possible corrosion risks of the employed Pipeline steels corresponding to the impurity Level of the gas source. Recent studies have shown that even the high alloyed materials might be susceptible to General and/or localized corrosion by the condensates forming from the impurities such as SOx, NOx, CO, O2 and water. Up to now, however, there is no regulation procedure which defines the maximum acceptable level of impurities and the combination of them for each employed pipeline steels. Herein, systematic experiment series were conducted by mixing pure CO2 gas with varying concentration of each impurity and with the varying combination of them. Each time, the mixture was then fed (1 L/min) into the reactor containing 12 specimens for 120-600 h at 5°C (to simulate the sub-level Pipeline transport). The resulted condensate was collected and analyzed by ionic chromatography and atomic Absorption spectroscopy to determine the chemical composition. In this study, the “worstcase scenario” gas mixture, containing 2.5 % H2O, 1.8 % O2, 1000 ppm NO2, and 220 ppm SO2 as impurities, resulted in the condensate containing H2SO4 0.114 M and HNO3 0.0184 M (pH 2.13). This “original” condensate was then reproduced to carry out exposure tests and electrochemical characterization including corrosion potentials and impedance spectroscopy in CO2 saturated condition for 7-14 days at the same temperature. The corrosion rate was also measured by mass loss method. We can conclude that, at the initial stage, HNO3 plays the dominant role in Fe dissolution process, while H2SO4 is responsible for the pit initiation followed by pitting corrosion. Future studies will be focused on the combination effect from the impurities and the exposure test under the regularly changing condensate to mimic the real CO2 pipeline system. T2 - Eurocorr 2016 CY - Montpellier, France DA - 11.09.2016 KW - Pipeline transport KW - Condensation KW - Corrosion KW - Carbon capture utilization KW - CO2 PY - 2016 AN - OPUS4-37752 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bäßler, Ralph A1 - Stoljarova, A. A1 - Regenspurg, S. T1 - Influence of Precipitating Brine Components on Materials Selection for Geothermal Applications N2 - Since geothermal wells are a feasible energy source to replace fossil fuel supply, many technologies have been developed to take advantage of geothermal energy. Nevertheless, service conditions in geothermal facilities are in many cases extreme in terms of corrosion due to the chemical composition of hydrothermal fluids and temperatures. Therefore, materials selection based on preliminary material qualification is essential to guarantee a secure and reliable operation of the facilities. During operation of a geothermal research facility in Groß Schönebeck copper and lead effects have been found downhole. Occurring mechanisms and measures to prevent precipitation or scaling needed to be investigated as well as potential influences of such precipitates on corrosion resistance of metallic materials used for equipment. This contribution deals with the evaluation of the corrosion behavior of carbon steel and corrosion resistant alloys in copper and/or lead containing artificial geothermal water, simulating the conditions in the Northern German Basin. The behavior of these materials in an artificial geothermal water obtained by electrochemical measurements and exposure tests are presented. While carbon steel exhibits precipitation and deposition, higher alloyed material shows different response to such species and a higher resistance in saline geothermal water. Basing on these results the suitability of the investigated corrosion resistant alloy is given for use in such conditions, whereas carbon steel creates difficulties due to its susceptibility to Cu- and Pb-precipitation. T2 - World Geothermal Congress CY - Online meeting DA - 30.03.2021 KW - Copper KW - Lead KW - Corrosion KW - Steel KW - Geothermal energy PY - 2021 SP - 1 EP - 11 AN - OPUS4-52828 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Özcan Sandikcioglu, Özlem T1 - High-throughput, automated and autonomous approaches for the design of corrosion resistant materials N2 - The integration of high-throughput electrochemistry, experimental automation and AI-driven processes is enabling the rapid discovery and optimization of advanced materials. This presentation will summarize our research in this field. T2 - GfKORR Grundlagen und Simulation Arbeitsgruppentreffen CY - Online meeting DA - 04.07.2024 KW - MAPs@BAM KW - CCMat KW - Corrosion KW - Electrochemistry PY - 2024 AN - OPUS4-62644 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Rütters, R. T1 - Towards defining reasonable minimum composition thresholds – impacts of variable CO2 stream compositions on transport, injection and storage N2 - The collaborative project “Impacts of impurities in CO2 streams captured from different emitters in a regional cluster on transport, injection and storage (CLUSTER)” aimed to set up recommendations on how to define “reasonable minimum composition thresholds” that CO2 streams should meet when accessing CO2 transport pipeline networks. Within CLUSTER, we investigated potential impacts of CO2 streams with different and temporally variable compositions and mass flow rates along the whole CCS chain. Investigations included, amongst others, impacts on: Corrosion of pipeline steel, pipeline network design and related transport costs, alteration of well bore cements, pressure evelopment and rock integrity, geochemical reactions, and petrophysical and geomechanical rock properties. All investigations are based on a generic CCS chain scenario. In this scenario, CO2 streams are captured from a spatial cluster of eleven emitters and collected in a regional pipeline network. Emitters comprise seven fossil fuel-fired power plants equipped with different capture technologies, two cement plants, one refinery and one integrated iron and steel plant. In total, 19.78 Mio t CO2 (including impurities) are captured in the emitter cluster annually. The combined CO2 stream is transported in a trunk line with a length of 400 km (100 km of these offshore) and is injected into five generic storage structures. The storage reservoirs are saline aquifers of the Buntsandstein. The investigations revealed beneficial and deteriorating impacts of different impurities and combinations thereof. Overall, no fundamental technical obstacles for transporting, injecting and storing CO2 streams of the modelled variable compositions and mass flow rates were observed. Based on the results, the CLUSTER project team recommends not to define “minimum composition thresholds” for CO2 streams as strict threshold values for eachindividual impurity in the stream. Instead, CO2 stream compositions and variabilities for specific CCS projects should be constrained with regard to a set of parameters including i) the overall CO2 content, ii) maximum contents of relevant impurities or elements, iii) acceptable variability of CO2 stream composition, and iv)impurity combinations to be avoided. T2 - 15th International Conference on Greenhouse Gas Control Technologies, GHGT-15 CY - Online meeting DA - 15.03.2021 KW - Corrosion KW - Impurities KW - CO2 quality KW - Pipeline network KW - Whole-chain CCS scenario KW - Recommendations PY - 2021 AN - OPUS4-52419 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Wetzel, Annica A1 - Morell, Daniel A1 - von der Au, Marcus A1 - Witt, Julia A1 - Özcan Sandikcioglu, Özlem T1 - Transpassive Behavior of Equimolar CrMnFeCoNi and CrCoNi Multi‐Principal Element Alloys in an Alkaline NaCl Electrolyte N2 - AbstractWe investigated the corrosion properties and transpassive behavior of CrMnFeCoNi and CrCoNi multi‐principal element alloys (MPEAs) in a 0.1 M NaCl electrolyte at pH 12. By using SECM‐based tip substrate voltammetry (TSV) in combination with the chemical analysis of the electrolyte, we were able to differentiate between anodic metal dissolution and oxygen evolution in the transpassive range. Our investigations have shown that CrCoNi has a significantly higher corrosion resistance compared to CrMnFeCoNi. In the studied alkaline environment, a transpassive oxide film is formed on the surface of CrCoNi during secondary passivation. This transpassive oxide film appears to play a significant role in oxygen evolution, as the increase in TSV currents at the microelectrode coincides with the corresponding current density plateau of the voltametric current trace. The formation of the transpassive oxide film was not observed in previous studies conducted in acidic environments. Moreover, the alkaline electrolyte induced a positive hysteresis and mild pitting corrosion, in addition to intergranular corrosion, which was the sole corrosion process observed at acidic pH levels. These findings enhance the understanding of the processes governing the transpassivity of CrMnFeCoNi and CrCoNi MPEAs in alkaline environments and have potential implications for the development of application‐tailored corrosion‐resistant MPEAs. KW - Multi-principal element alloys KW - MPEA KW - Corrosion KW - Oxygen evolution reaction KW - Transpassive region PY - 2024 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-611594 DO - https://doi.org/10.1002/celc.202400346 SN - 2196-0216 SP - 1 EP - 9 PB - Wiley AN - OPUS4-61159 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Koerdt, Andrea T1 - Microbial corrosion of iron coupled to methanogenesis by strains from different environments N2 - Microbially influenced corrosion (MIC) of iron is usually attributed to sulfate-reducing microorganisms (SRM) which act upon the metal by the reactiveness of hydrogen sulfide, and by withdrawal of the available electrons in electrical contact with the metal. Methanogenic archaea are supposed to cause MIC. Because they do not produce hydrogen sulfide, withdrawal of electrons may be their main corrosive mechanism; however, mechanistic details and kinetics of the overall process are poorly understood. Precipitation of siderite (4Fe + 5HCO3 + 5H+  4FeCO3 + CH4 + 3H2O) can lead to an insulating layer on the metal surface and lower the corrosion rate. Still, the extent of FeCO3 precipitation may be significantly influenced by environmental conditions such as pH and advective processes. T2 - EMBO-Workshop CY - Vienna, Austria DA - 02.08.2018 KW - Methanogens KW - MIC KW - Corrosion KW - Environmental Simulation PY - 2018 AN - OPUS4-46396 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bäßler, Ralph T1 - Metallic Materials for Geothermal Applications N2 - The aim of the work presented was the evaluation of corrosion resistance of various materials in geothermal Waters as a base to create a catalogue of suitable materials for applications in (not only) German geothermal power plants. Users shall be enabled to have a basis for designing such facilities. High alloyed corrosion resistant alloys are suitable and do not cause copper or lead deposition. They shall be chosen for future design of the piping system, either in massive or in cladded form, if crevices formation with non-metallic materials can be prevented! T2 - IFPEN-Workshop: Corrosion in Low-Carbon Energies CY - Online meeting DA - 03.11.2020 KW - Geothermal KW - Corrosion KW - Saline brine PY - 2020 AN - OPUS4-51511 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Aristia, Gabriela A1 - Le, Quynh Hoa A1 - Bäßler, Ralph T1 - Effect of CO2 gas on carbon steel corrosion in an acidic-saline based geothermal fluid N2 - Geothermal energy is one of the most promising energy resources to replace fossil fuel. To extract this energy, hot fluids of various salts and gases are pumped up from a geothermal well having a certain depth and location. Geothermal wells in volcanic regions often contain highly corrosive CO2 and H2S gases that can be corrosive to the geothermal power-plants, which are commonly constructed of different steels, such as carbon steel. This research focuses on the corrosion behaviour of carbon steel exposed to an artificial geothermal fluid containing CO2 gas, using an artificial acidic-saline geothermal brine as found in Sibayak, Indonesia. This medium has a pH of 4 and a chloride content of 1,500 mg/L. Exposure tests were conducted for seven days at 70 °C and 150 °C to simulate the operating temperatures for low and medium enthalpy geothermal sources. Surface morphology and cross-section of the specimens from the above experiments were analysed using scanning electron microscope (SEM) and energy dispersive X-ray (EDX). Electrochemical tests via open circuit potential (OCP) and electrochemical impedance spectroscopy (EIS) were performed to understand the corrosion processes of carbon steel in CO2-containing solution both at 70 °C and 150 °C. Localized corrosion was observed to a greater extent at 70 °C due to the less protectiveness of corrosion product layer compared to that at 150 °C, where FeCO3 has a high corrosion resistance. However, a longer exposure test for 28 days revealed the occurrence of localized corrosion with deeper pits compared to the seven-day exposed carbon steel. In addition, corrosion product transformation was observed after 28 days, indicating that more Ca2+ cations incorporate into the FeCO3 structure. T2 - EUROCORR 2019 CY - Sevilla, Spain DA - 09.09.2019 KW - Carbon steel KW - CO2 KW - EIS KW - Geothermal KW - Corrosion PY - 2019 SP - Paper 200245, 1 EP - 5 CY - Madrid, Spain AN - OPUS4-49099 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Le, Quynh Hoa T1 - On the corrosion behaviour of CO2 injection pipe steels: Role of cement N2 - Carbon Capture and Storage (CCS) is identified as an excellent technology to reach the target of CO2 reduction. However, the safety issue and cost-effectiveness hinder the future of CCS. For the reliability and safety issues of injection wells, the corrosion resistance of the materials used needs to be determined. In this study, representative low-cost materials including carbon steel 1.8977 and low alloyed steel 1.7225 were investigated in simulated pore water at 333 K and under CO2 saturation condition to represent the worst-case scenario: CO2 diffusion and aquifer fluid penetration. These simulated pore waters were made from relevant cement powder to mimic the realistic casing-cement interface. Electrochemical studies were carried out using the pore water made of cement powder dissolved in water in comparison with those dissolved in synthetic aquifer fluid, to reveal the effect of cement as well as formation water on the steel performance. Two commercially available types of cement were investigated: Dyckerhoff Variodur® and Wollastonite. Variodur® is a cement containing high performance binder with ultra-fine blast furnace slag which can be used to produce high acid resistance concrete. On the other hand, Wollastonite is an emerging natural material mainly made of CaSiO3 which can be hardened by converting to CaCO3 during CO2 injection. The results showed the pH-reducing effect of CO2 on the simulated pore water/aquifer (from more than 10 to less than 5) leading to the active corrosion process that happened on both 1.8977 and 1.7225. Electrochemical characterization showed negative free corrosion potential and polarisation curves without passive behaviors. The tested coupons suffered from pitting corrosion, which was confirmed by surface analysis. Interestingly, basing on the pit depth measurements from the tested coupons and the hardness of cement powder, it is suggested that Variodur® performed better than Wollastonite in both aspects. The electrochemical data was compared to that resulted from exposure tests to give a recommendation on material selection for bore-hole construction. T2 - EUROCORR 2019 CY - Sevilla, Spain DA - 09.09.2019 KW - Carbon capture KW - Utilization, and storage (CCUS) technology KW - Corrosion KW - Carbon steel KW - Mortel KW - Crevice corrosion PY - 2019 AN - OPUS4-49105 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Pötzsch, Sina T1 - Resistance of metals exposed to heating oil blends with 10 % and 20 % biodiesel (FAME) N2 - In Europe biodiesel gained from rapeseeds are considered as an alternative to common fossil fuels due to its environmental performance and its independence from import of raw materials. Biodiesel is also suitable to serve as blending component to heating oil. In that case, it must be considered that changes of fuel composition might cause material degradation. The objective of this research was to investigate the resistance of metallic materials exposed to heating oil, heating oil blend B20 with 20 % biodiesel and pure biodiesel. Furthermore, the resistance of metals to eight-year aged B10 and six-year aged pure biodiesel was evaluated. Ageing of biodiesel forms acids and water which might propagate metal corrosion. The investigated metals (aluminium, unalloyed steel, austenitic CrNi-steel, copper, die cast zinc and brass) are commonly used for components in middle distillate facilities. According to DIN 50905-4 the immersed metals were exposed in a climate chamber at 50°C for 4 weeks. The metallic materials were evaluated as resistant if the annual corrosion rate due to uniform corrosion remained under 0.1 mm/year and no localized corrosion in the form of pitting occurred. The corrosion rates of the exposed materials stayed far below the limit of 0.1 mm/year for all tested fuels. An exception was die cast zinc ZP0410 in eight-year aged B10; a corrosion rate up to 0.3 mm/year due to uniform corrosion was measured. In no case localized corrosion occurred. Copper and brass caused discolouration of biodiesel from yellow to green. In conclusion, the tested metallic materials were resistant in heating oil, heating oil blend B20 and pure biodiesel at 50 °C. Even the metals exposed to six-year aged biodiesel and eight-year aged B10 showed no uniform or localized corrosion; except for zinc, which was not resistant in eight-year aged B10. T2 - EUROCORR 2019 CY - Sevilla, Spain DA - 09.09.2019 KW - Metals KW - Heating oil KW - Biodiesel KW - RME KW - Corrosion KW - Compatibility KW - FAME PY - 2019 AN - OPUS4-49137 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Schütter, Jan T1 - Effect of surface topography and chemistry on the attachment of bacteria on solid surfaces N2 - Microbiologically induced corrosion due to bacterial biofilms causes several problems in industrial systems, technical applications and in medicine. Prior to the formation of a biofilm on a substrate, planktonic cells attach on the surface. Hence, the properties of the surface play a key role in biofilm formation and are of great importance for the development of strategies to prevent bacterial attachment and biofilm formation. This project aims at clarifying to which extent surface micro-/nanostructuring and chemical functionalization affects bacterial attachment and whether a synergistic combination of the two can be used to control bacterial adhesion. To answer these questions, model surfaces with regular patterns of 5-10 micrometers in size have been prepared, which provide distinct zones differing in terms of their chemistry or nano-roughness. This was achieved by micro contact printing of self-assembled monolayers with different functional groups and deposition of patterned ZnO nanorod arrays for studying the effect of surface chemistry and morphology, respectively. Typical contrasts studied were combinations of positively/negatively charged, hydrophobic/hydrophilic or flat/rough. The attachment behavior of bacteria on tailored surfaces were studied in a flow chamber as a function of time. The strain Pseudomonas fluorescens SBW25 was chosen as a model organism. DNA-intercalating dyes such as Syto9 have a high affinity to adsorb on ZnO nanorods. To overcome this limitation a genetic modification was performed by introducing a gene which expresses a green fluorescent protein in P. fluorescens SBW25 enabling the quantitative evaluation of the flow chamber studies by means of fluorescence microscopy. Further analysis of the attachment behavior was performed by means of scanning electron microscopy. The presentation will summarize the results of our systematic study on the role of individual parameters on bacterial attachment and highlight synergistic combinations, showing an inhibition or enhancing effect. As the investigations with model substrates enable a precise control of the surface parameters, this approach can be applied to different microorganisms and material systems to achieve a correlative description of bacterial adhesion on solid surfaces. T2 - Eurocorr2019 CY - Sevilla, Spain DA - 09.09.2019 KW - Microbial KW - Corrosion KW - MIC KW - Nanorods PY - 2019 AN - OPUS4-49730 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Aristia, Gabriela T1 - Fenomena Korosi pada aplikasi panas bumi N2 - To accelerate the development of Indonesian geothermal energy, progress should be done in all aspects. Corrosion is an important part on the technological development to ensure the safety and longevity of a power plant. T2 - Fireside Chat der Indonesischen Botschaft CY - Berlin, Germany DA - 21.11.2019 KW - Corrosion KW - Korosi KW - Korrosion PY - 2019 AN - OPUS4-49735 LA - mul AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Özcan Sandikcioglu, Özlem T1 - Application of atomic force microscopy (AFM) for in situ corrosion studies of thin film covered AA2024 T3 aluminium alloy surface N2 - The performance of functional coatings and adhesively joined hybrid components relies strongly on the stability of the polymer-metal interface. With the increasing utilization of multi-material structures in the automotive and aerospace industry, it is of great scientific and technical interest to understand the processes leading to interface degradation and to develop novel strategies to increase corrosion and delamination resistance. The aim of this project is to develop thin epoxy-based films and their carbon nanofiller loaded composites on aluminium alloy AA2024-T3 as a model system and to investigate their interfacial stability under corrosive and coupled corrosive-mechanical load. Spin coating was used for the layer-by-layer deposition of poly[(o-cresyl glycidyl ether)-co-formaldehyde] and poly-(ethylenimine) bi-layers. Atomic force microscopy (AFM) results indicate a very homogeneous and dense film with low surface roughness. Carbon nanofillers were introduced either by mixing into the coating components or in between individual layers to control the separation between the carbon nanofillers and alloy surface. The film chemistry and barrier properties were characterized by means of spectroscopic and electrochemical methods, respectively. The degradation and delamination behavior of the epoxy-based films was characterized by means of in situ AFM corrosion experiments. The quantitative imaging (QI) mode allowed the observation of hydrogen-generation induced blister formation during exposure to corrosive electrolyte and how the local corrosion processes evolved with exposure time. Complementary energy dispersive X-ray spectroscopy (EDX) analysis was performed to correlate the corrosion behavior with the different intermetallic particle chemistries and distributions. The presentation will summarize our results on the effect of interface chemistry and carbon nanofiller – alloy separation on the initiation of local corrosion processes on thin film covered AA2024-T3 aluminium alloys. T2 - EuroCorr2019 CY - Sevilla, Spain DA - 09.09.2019 KW - Corrosion KW - Atomic Force Microscopy (AFM) PY - 2019 AN - OPUS4-50293 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Özcan Sandikcioglu, Özlem T1 - In situ atomic force microscopy (AFM) analysis of materials under combined corrosive and mechanical load N2 - In service, most materials are operated under simultaneous corrosive and mechanical load and there are very few methods capable for testing material degradation under these conditions, especially when it comes to high resolution analysis. For this purpose, in this work, a tensile module capable of uniaxial stretching and compression with up to 5 kN force was integrated into an AFM stage. The elimination of the need for sample unmounting and remounting and the resulting possibility of keeping the sample under constant mechanical load during AFM measurements not only enables a precise positioning of the area of interest but also allows for the analysis of processes in the elastic deformation regime. This methodology was demonstrated for two case studies. Scanning Kelvin Probe Force Microscopy (SKPFM) was used as the main tool to characterize the deformation behavior. Moreover, a flexible electrochemical measurement cell was used to enable electrochemical analysis by means of electrochemical impedance spectroscopy (EIS) and Linear Sweep Voltammetry (LSV) during AFM measurements at different levels of strain. The in situ AFM results are complemented by microstructure analysis by means of electron backscatter diffraction (EBSD). In the first case study, the deformation induced delamination of a thin organic coating on AA2024 T3 aluminium alloy was investigated as a function of alloy surface treatment. The formation of cracks in the insulating passive film enabled an early detection of deformation processes by means of SKPFM. The second case study focused on the comparison of corrosion and deformation behavior of conventional and additively manufactured 316 stainless steels. In comparison to the conventional 316 stainless steel, the effect of processing was clearly detectable on the additively manufactured material as zones of inhomogeneous potential, which also affected the initiation of local corrosion processes. The contribution will provide detailed information on the new AFM setup and summarize our results from both case studies. T2 - EuroCorr2019 CY - Sevilla, Spain DA - 09.09.2019 KW - Corrosion KW - Coupled corrosive and mechanial load KW - Atomic Force Microscopy (AFM) PY - 2019 AN - OPUS4-50294 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Bäßler, Ralph T1 - Review: Materials Handbook–A Concise Desktop Reference N2 - This concise reference book,consisting of 2 volumes, provides “key scientific and technical properties and data” for “materials scientists, metallurgists, engineers,chemists, and physicists as well as academic staff, technicians, and students” dealing with such kind of materials. Within its 3rd edition the previous work was extended by a chapter on occupational health and safety issues of materials, beside of the update of whole content. Within 22 chapters materials properties and data are summarized in many tables. Some facts are illustrated by drawings and diagrams for better understandability. Each chapter ends with a part on further reading arranged accordingly. KW - Corrosion KW - Materials KW - Corrosivity KW - Resistance PY - 2020 DO - https://doi.org/10.1002/maco.202070034 SN - 1521-4176 SN - 0947-5117 VL - 71 IS - 3 SP - 509 PB - WILEY‐VCH Verlag GmbH & Co. KGaA CY - Weinheim AN - OPUS4-50489 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Seifert, Lando T1 - Review: Concrete Repair to EN 1504: Diagnosis, Design, Principles and Practice N2 - In 2019 CRC Press published the “Concrete Repair to EN 1504” as paperback. This issue does not differ in terms of content from the hardback publication of 2014. Like the previous version, the book covers both detailed background information on repair procedures of reinforced concrete structures and provides a reference work for technicians and people who are involved with the maintenance of these structures, according to EN 1504. The book presents a high number of figures and tables, i.e., approximately one illustration per page. For readers who prefer a more comfortable to handle paperback, the book is recommended; however, the hardback from 2014 is still up‐to‐date. KW - Corrosion KW - Concrete KW - Bridge PY - 2020 DO - https://doi.org/10.1002/maco.202070064 SN - 1521-4176 SN - 0947-5117 VL - 71 IS - 6 SP - 1036 PB - WILEY‐VCH Verlag GmbH & Co. KGaA CY - Weinheim AN - OPUS4-50838 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Le, Quynh Hoa T1 - CO2-stream impurities and their effects on corrosion susceptibility of materials to be used in CCUS systems N2 - Carbon Capture Utilization and Storage (CCUS) is a promising technology to reach the target for reduction of CO2 emissions. Crucial points for a sustainable and future-proof CCUS system are reliability and cost efficiency of the whole process chain, including separation of CO2 from the source, compression of CO2, its subsequent transportation to the injection site and injection into geological formations, e.g. aquifers. Recent studies have shown that even at a very low concentration of impurities, condensation of sulfuric and nitric acids in dense phase CO2 are possible and observable. Thus, impact of impure CO2 stream toward corrosion susceptibility of materials to be used in CCUS system need to be considered. In this talk, basing on results achieved from two German long-term projects (COORAL and CLUSTER), the dominating impurities of the CO2 stream and corrosion mechanisms are addressed. Investigations cover the whole CCUS process chain and provide a material recommendation for certain parts. T2 - Corrosion in Low-Carbon Energies - IFPEN-Lyon CY - Online meeting DA - 03.11.2020 KW - Corrosion KW - CCUS KW - Carbon dioxide PY - 2020 AN - OPUS4-51509 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Bäßler, Ralph T1 - Review: Corrosion of Linings and Coatings: Cathodic and Inhibitor Protection and Corrosion Monitoring N2 - This paperback issue of the 2007 hardcover version within the “Corrosion Engineering Handbook” series presents various materials and methods for controlling and protecting against corrosion instead of using expensive alloys to construct a tank or processing vessel. This book is a very comprehensive collection of the current knowledge about applied linings and coatings. So, it fulfills its intension, “that regardless of what is being built, … information for … whoever is responsible for the selection of material of construction will be found in this book to enable them to avoid unnecessary loss of material through corrosion”, to a very large extent. KW - Corrosion KW - Coating KW - Lining KW - Cathodic protection PY - 2020 DO - https://doi.org/10.1002/maco.202070104 SN - 1521-4176 SN - 0947-5117 VL - 71 IS - 10 SP - 1756 EP - 1757 PB - WILEY‐VCH Verlag GmbH & Co. KGaA CY - Weinheim AN - OPUS4-51414 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Bäßler, Ralph T1 - Review: Materials Informatics -Metals, Tools and Applications N2 - Since data processing has now also found its way into materials science, there has been a great demand from users for a corresponding textbook. This book provides a guide to the latest advances of materials informatics and data mining for materials science. 46 authors introduce readers to methods, present tools and case studies to illustrate the power of materials informatics within this new field of application. KW - Corrosion KW - Materials behavior PY - 2020 DO - https://doi.org/10.1002/maco.202070114 SN - 1521-4176 SN - 0947-5117 VL - 71 IS - 11 SP - 1928 EP - 1929 PB - WILEY‐VCH Verlag GmbH & Co. KGaA CY - Weinheim AN - OPUS4-51513 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Aristia, Gabriela A1 - Bäßler, Ralph A1 - Roth, C. T1 - Polyaniline/silicon dioxide containing coating for use in artificial geothermal brines N2 - Geothermal brine is a complex system containing a wide variety of dissolved salts resulting from the condition s in a geothermal well. These fluids lead to corrosion in pipes and other parts of geothermal system construction and necessitate intense research efforts in finding new suitable materials. Carbon steel is susceptible to corrosion in geothermal brine especially when it is exposed to a high temperature and high-pressure medium, which is considered to be an aggressive environment. An artificial geothermal water, bas ed on a brine composition found in Indonesia, was used to investigate the performance of high alloyed materials. The electrolyte has pH 4 and contains 1,500 mg/l Cl-, 20 mg/l SO4 2-, 15 mg/l HCO3 -, 200 mg/l Ca 2+, 250 mg/l K+, and 600 mg/l Na+. In order to protect the bare material in geothermal application, it is necessary to either use high alloyed material s or coatings. In this research, a coating system consisting of polyaniline and silicon dioxide was investigated regarding its behavior to protect carbon steel. In detail, the effect of SiO2 and polyaniline (PANi) addition was evaluated by exposure and electrochemical tests for 7 days, i.e. electrochemical impedance spectroscopy (EIS) and open circuit potential (OCP ) at room temperature and 150 °C with 1 MPa pressure . T2 - NACE International Annual Corrosion Conference CY - Phoenix, AZ, USA DA - 15.04.2018 KW - Geothermal KW - Coating KW - SiO 2 KW - Polyaniline KW - Corrosion PY - 2018 SP - 10708, 1 EP - 14 PB - Omnipress CY - Houston AN - OPUS4-44916 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Aristia, Gabriela A1 - Le, Quynh Hoa A1 - Bäßler, Ralph T1 - Study of Polyaniline/Silicon Dioxide based Coating on Carbon Steel in Artificial Geothermal Brine N2 - Geothermal brines are corrosive in nature because of their salt contents and high temperatures. Therefore, they pose a major challenge to geothermal power-plants, which are mostly built of low alloyed steels, e.g., carbon steel. Carbon steel is susceptible to uniform and localized corrosion when exposed to geothermal brines having acidic-saline properties. To overcome this limitation, geothermal power plants should be built by either high alloyed materials or by integrating protection systems on carbon steel, such as coatings and inhibitors. We studied a coating system containing polyaniline/silicon dioxide basing on locally available resources that provides protection against corrosion of carbon steel and enhance the thermal resistance in geothermal environments. Here, exposure and electrochemical tests of coated carbon steels were performed in an artificial geothermal brine. The solution had a pH of 4, with the composition of 1,500 mg/L of chlorides, which is based on the chemical analysis of geothermal brine found in Sibayak, Indonesia. All exposure tests were conducted using autoclaves at 150 °C with a total pressure of 1 MPa, which was performed for up to six months to evaluate the durability of the coating system. Post-experimental analyses were performed by assessing the surface of specimens using optical and electron microscopes. On the other hand, electrochemical tests were performed for seven days at 25 °C and 150 °C to investigate the kinetics of electrochemical reactions by measuring open circuit potential and electrochemical impedance spectra. Experimental results showed the corrosion resistance of PANI/SiO2 composite coatings, where polyaniline and SiO2 play their roles as stabilizers. T2 - World Geothermal Congress CY - Online meeting DA - 30.03.2021 KW - Coatings KW - Corrosion KW - Polyaniline KW - Sibayak KW - SiO2 PY - 2021 SP - 1 EP - 7 AN - OPUS4-52830 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - An, Biwen Annie A1 - Shen, Y. A1 - Voordouw, J. A1 - Voordouw, G. T1 - Halophilic methylotrophic methanogens may contribute to the high ammonium concentrations found in shale oil and shale gas reservoirs N2 - Flow-back and produced waters from shale gas and shale oil fields contain high ammonium, which can be formed by methanogenic degradation of methylamines into methane and ammonium. Methylamines are added to fracturing fluid to prevent clay swelling or can originate from metabolism of the osmolyte triglycinebetaine (GB). We analyzed field samples from a shale gas reservoir in the Duvernay Formation and from a shale oil reservoir in the Bakken formation in Canada to determine the origin of high ammonium. Fresh waters used to make fracturing fluid, early flow-back waters, and late flow back waters from the shale gas reservoir had increasing salinity of 0.01, 0.58, and 2.66 Meq of NaCl, respectively. Microbial community analyses reflected this fresh water to saline transition with halophilic taxa including Halomonas, Halanaerobium, and Methanohalophilus being increasingly present. Early and late flow-back waters had high ammonium concentrations of 32 and 15 mM, respectively. Such high concentrations had also been found in the Bakken produced waters. Enrichment cultures of Bakken produced waters in medium containing mono, di-, or trimethylamine, or triglycinebetaine (GB) converted these substrates into ammonium (up to 20 mM) and methane. The methylotrophic methanogen Methanohalophilus, which uses methylamines for its energy metabolism and uses GB as an osmolyte, was a dominant community member in these enrichments. Halanaerobium was also a dominant community member that metabolizes GB into trimethylamine, which is then metabolized further by Methanohalophilus. However, the micromolar concentrations of GB measured in shale reservoirs make them an unlikely source for the 1,000-fold higher ammonium concentrations in flow-back waters. This ammonium either originates directly from the reservoir or is formed from methylamines, which originate from the reservoir, or are added during the hydraulic fracturing process. These methylamines are then converted into ammonium and methane by halophilic methylotrophic methanogens, such as Methanohalophilus, present in flow-back waters. KW - Methanogen KW - Oil and gas industry KW - Shale KW - Halophile KW - Corrosion PY - 2019 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-474982 DO - https://doi.org/10.3389/fenrg.2019.00023 SN - 2296-598X VL - 7 SP - 1 EP - 13 PB - Frontiers Media CY - Lausanne AN - OPUS4-47498 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Koerdt, Andrea T1 - Investigation of methanogen-induced microbiologically influenced corrosion (Mi-MIC) using simulated marine environments under flowing conditions N2 - Microbiologically influenced corrosion (MIC) of iron is usually attributed to sulfate-reducing microorganisms (SRM) in offshore industries, such as the oil and gas pipelines, due to the high concentrations of sulfate in the seawater. SRM act upon the metal by the reactiveness of hydrogen sulfide (HS-), and by withdrawal of the available electrons (Fe --> Fe2+ + 2e-; E° = -0.47 V) in electrical contact with the metal (EMIC). However, methanogenic archaea can also cause MIC. Because they do not produce HS-, withdrawal of electrons may be their main corrosive mechanism; however, mechanistic details and kinetics of the overall process are poorly understood. To investigate the corrosion potential of methanogens, we studied the EMIC methanogenic strains isolated from marine sediments (Methanobacterium-affiliated strain IM1) and crude oil tanks (Methanococcus maripaludis Mic1c10), in an in-house developed flow-through cell to simulate a fluctuating environment. A co-culture of M. maripaludis and D. alaskensis was also established to study the effect of syntrophic growth on metal corrosion that may occur in industrial pipelines. Results indicate that the rates of iron corrosion due to coupled methanogenesis (up to 0.4 mm/yr) are higher to that caused by the marine SRM Desulfovibrio alaskensis (0.15 mm/yr). Surface analyses of the metal showed severe pitting with high methane production. Genomic analysis of the EMIC methanogen M. maripaludis Mic1c10 will provide an insight on the mechanisms of MIC. Such knowledge and deeper understanding also from an electrokinetic point of view may not only provide further models in microbial electrophysiology, but also contribute to mitigation strategies in MIC T2 - Einladung zum Kolloquium HZDR – Helmholtz-Zentrum Dresden-Rossendorf CY - Dresden, Germany DA - 24.09.2019 KW - Corrosion KW - MIC KW - Archaea KW - Methanogens KW - Environmental Simulation PY - 2019 AN - OPUS4-49403 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Koerdt, Andrea T1 - Investigation of methanogen-induced microbiologically influenced corrosion (Mi-MIC) using simulated marine environments under flowing conditions N2 - Microbiologically influenced corrosion (MIC) of iron is usually attributed to sulfate-reducing microorganisms (SRM) in offshore industries, such as the oil and gas pipelines, due to the high concentrations of sulfate in the seawater. SRM act upon the metal by the reactiveness of hydrogen sulfide (HS-), and by withdrawal of the available electrons (Fe --> Fe2+ + 2e-; E° = -0.47 V) in electrical contact with the metal (EMIC). However, methanogenic archaea can also cause MIC. Because they do not produce HS-, withdrawal of electrons may be their main corrosive mechanism; however, mechanistic details and kinetics of the overall process are poorly understood. To investigate the corrosion potential of methanogens, we studied the EMIC methanogenic strains isolated from marine sediments (Methanobacterium-affiliated strain IM1) and crude oil tanks (Methanococcus maripaludis Mic1c10), in an in-house developed flow-through cell to simulate a fluctuating environment. A co-culture of M. maripaludis and D. alaskensis was also established to study the effect of syntrophic growth on metal corrosion that may occur in industrial pipelines. Results indicate that the rates of iron corrosion due to coupled methanogenesis (up to 0.4 mm/yr) are higher to that caused by the marine SRM Desulfovibrio alaskensis (0.15 mm/yr). Surface analyses of the metal showed severe pitting with high methane production. Genomic analysis of the EMIC methanogen M. maripaludis Mic1c10 will provide an insight on the mechanisms of MIC. Such knowledge and deeper understanding also from an electrokinetic point of view may not only provide further models in microbial electrophysiology, but also contribute to mitigation strategies in MIC T2 - Archaea Meeting-Schmitten VAAM Fachgruppe CY - Schmitten, Germany DA - 12.09.2019 KW - Corrosion KW - MIC KW - Archaea KW - Methanogens KW - Environmental Simulation PY - 2019 AN - OPUS4-49405 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Erning, Johann Wilhelm T1 - Observations of copper pitting corrosion in german tap waters N2 - In recent years, a new type of pitting corrosion is observed on half-had copper pipes. examples are given and possible reasons are discussed T2 - Eurocorr 2019 CY - Sevilla, Spain DA - 09.09.2019 KW - Water KW - Pitting KW - Corrosion KW - Copper KW - Drinking PY - 2019 AN - OPUS4-49281 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Erning, Johann Wilhelm T1 - A new type of copper pitting corrosion in german tap waters N2 - Half-hard copper pipes show pitting corosion under conditions until now seen as uncritical. Examples are discussed, possible causes described. T2 - MTECH 2019 CY - Porec, Croatia DA - 09.10.2019 KW - Drinking KW - Pitting KW - Corrosion KW - Copper KW - Water PY - 2019 AN - OPUS4-49283 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - An, Biwen Annie T1 - Microbial modelling of sulfate-reducing bacteria (SRB) and methanogenic archaea (ME) using iron N2 - Sulfate reducing bacteria (SRB) and methanogenic archaea (MA) are commonly found in the oil and gas environments. The formation of hydrogen sulfide (HS-) is particularly concerning for the petroleum industry due to its corrosiveness. However, the activities of SRB are limited to the concentration of sulfate present in the environment, whereas methanogens can utilize substrates such as H¬2 for methanogenesis. MA is commonly found in sulfate-free environments, such as deep sediments, and are known to form interspecies electron transfer relationships with SRB. Recently, SRB and MA capable of microbiologically influenced corrosion (MIC) by using elemental iron as a direct electron source (EMIC) have gained increased attention. On the iron surface, EMIC-SRB can outcompete EMIC-MA in the presence of sulfate, but this changes as sulfate depletes. The formation of FeS on the metal surface can be further utilized by MA for methanogenesis as it provides a conductive path. However, the possible kinetics involved of the overall process are currently unknown. We obtained a co-culture of EMIC-SRB and EMIC-MA to investigate the growth rates and electrical potential changes under different environmental conditions, including changes in pH, temperature and salinity. Results indicate that under neutral conditions and using iron as the sole substrate, methane production (up to 5 mM) starts after sulfate was depleted. Electrochemical measurements will be conducted on the co-culture under different conditions to determine the changes in the electrical potential in correlation with the sulfate and methane concentration. Fluorescence and electron microscope images of the biofilm structure will be used to visualize cell distribution and morphology. This study embarks the first step of understanding the relationship between EMIC-SRB and EMIC-MA. Such knowledge is important for the field of microbial electrophysiology and can be further explored for industrial applications. T2 - 7th International Symposium on Applied Microbiology and Molecular Biology in Oil Systems (ISMOS-7) CY - Halifax, Canada DA - 18.06.2019 KW - MIC KW - Corrosion KW - FIB/SEM KW - Corrosion products KW - Bacteria KW - Archaea KW - Iron PY - 2019 AN - OPUS4-49420 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Aristia, G. A1 - Le, Quynh Hoa A1 - Bäßler, Ralph A1 - Roth, C. T1 - The Effect of Different Polyaniline Types in Silicon Dioxide Containing Coatings for Carbon Steel Protection in Artificial Geothermal Brines N2 - According to the results of the experiments carried out, the following points can be concluded: 1. Exposure tests showed that specimens with the addition of SiO2 particles and polyaniline particles exhibit better corrosion resistance than specimens with the addition of only polyaniline particles or binder only. 2. Open circuit potential measurements showed that in the beginning of the experiments, both coatings had an open circuit potential 100 mV higher than carbon steel. Within one day of immersion, the potential of carbon steel increased significantly, indicating the formation of oxide layer. After extended exposure the carbon steel potential sat between PS1 (which had higher potential) and PS2 (which had a lower potential) and all three were in the range –600 mV to –500 mV vs Ag/AgCl. 3. Both coatings PS-1 and PS-2 were degraded with increasing exposure time, shown by the decrease of absolute impedance value at low frequency range after 2, 4, and 6 days exposure. 4. Potentiodynamic test was performed after 3 hours and 6 days exposure, and it was shown that the coating in the initial stage exhibited more passive behavior than the specimens exposed for 6 days. T2 - NACE International Corrosion Conference 2019 CY - Nashville, TN, USA DA - 24.03.2019 KW - Geothermal KW - Coating KW - Polyaniline KW - Corrosion PY - 2019 SP - 13121-1 EP - 13121-14 PB - NACE International CY - Houston AN - OPUS4-47913 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Falk, Florian T1 - The impact of water vapour on high-temperature surface degradation by sulfurous gases of ferritic alloys N2 - Sulfur and water have a fundamental impact on the corrosion rate and potential failure of materials. It is therefore necessary to understand the mechanisms, rates, and potential means of transport, as well as the reactions of these elements with an alloy. This work investigates the effect of water vapor in the initial stages of SO2 corrosion of an ferritic model alloy containing 9 wt% Cr and 0.5 wt% Mn. The exposure experiments were studied at 650°C in situ under laboratory conditions using energy-dispersive x-ray diffraction analysis. Two separate experiments were run, one with a 99.5% Ar + 0.5% SO2 atmosphere and one with a 69.5% Ar + 0.5% SO2 + 30% H2O atmosphere. With a wet atmosphere, the alloy formed a scale with decreasing oxygen content towards the scale–alloy interface. Sulfides were identified above and below a (Fe, Cr)3O4 layer in the inner corrosion zone. In contrast to this, the overall scale growth was slower in a dry SO2 atmosphere. T2 - EUROCORR CY - Barceló Sevilla Renacimiento, Seville, Spain DA - 09.09.2019 KW - Diffraction KW - Sulfidation KW - Early oxidation KW - Corrosion KW - In situ PY - 2019 AN - OPUS4-49213 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Falk, Florian T1 - Microstructural impact on high temperature oxidation behavior of Fe-Cr-C model alloys N2 - Chromia forming high alloyed ferritic-austenitic steels are being used as boiler tube materials in biomass and coal-biomass co-fired power plants. Despite thermodynamic and kinetic boundary conditions, microstructural features such as grain orientation, grain sizes or surface deformation contribute to the oxidation resistance and formation of protective chromium-rich oxide layers. This study elucidates the impact of microstructure such as the grain size and number of carbide precipitates on high temperature oxidation at 650°C in 0.5% SO2 atmosphere. Cold-rolled Fe-16Cr-0.2C material was heat-treated to obtain two additional microstructures. After exposure to hot and reactive gases for 10 h < t < 1000 h layer thicknesses and microstructure of oxide scales are observed by scanning electron microscopy and Energy-dispersive X-ray spectroscopy. The two heat treated alloys showed reasonable oxidation resistance after 1000 h of exposure. The oxidation rate was substantially higher for the alloy with a duplex matrix after heat treatment compared to the fine-grained material. T2 - Gordon Research Conference CY - New London, New Hampshire, USA DA - 21.07.2019 KW - Corrosion KW - Microstructure KW - Oxidation KW - Sulfidation PY - 2019 AN - OPUS4-49212 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Kamaraj, Abinaya A1 - Erning, Johann Wilhelm A1 - Reimann, S. A1 - Ahrens, A. T1 - Susceptibility of 304 stainless steel to crevice corrosion in electrochemically active fluids N2 - The susceptibility of AISI 304 stainless steel to crevice corrosion on the effect of contact with electrochemically active fluids was investigated using exposure and stepwise potentiostatic polarisation. Crevice materials made up of 304 SS and Polyether ether ketone (PEEK) forming two kinds of crevices including 304 SS-to-PEEK and 304 SS-to-304 SS were tested. T2 - NACE International Corrosion Conference 2019 CY - Nashville, TN, USA DA - 24.03.2019 KW - Steel KW - Crevice KW - Corrosion KW - ECA KW - Stainless PY - 2019 SP - Paper 12868 PB - NACE International CY - Houston AN - OPUS4-49286 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Erning, Johann Wilhelm T1 - Susceptibility of 304 stainless steel to crevice corrosion in electrochemically active fluids N2 - The susceptibility of AISI 304 stainless steel to crevice corrosion on the effect of contact with electrochemically active fluids was investigated using exposure and stepwise potentiostatic polarisation. Crevice materials made up of 304 SS and Polyether ether ketone (PEEK) forming two kinds of crevices including 304 SS-to-PEEK and 304 SS-to-304 SS were tested. T2 - Eurocorr 2019 CY - Sevilla, Spain DA - 09.09.2019 KW - ECA KW - Crevice KW - Corrosion KW - Stainless KW - Steel PY - 2019 AN - OPUS4-49282 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Pfennig, A. A1 - Kranzmann, Axel T1 - Corrosion and Fatigue of Heat Treated Martensitic Stainless Steel 1.4542 used for Geothermal Applications N2 - During capture and storage technology (CCS) as well as in geothermal energy production Steels need to withstand the corrosive environment such as: heat, pressure, salinity of the aquifer and CO2-partial pressure. 1.4542 shows unusual corrosion phenomena, but is still sufficiently resistant in corrosive environments. To better understand its behaviour differently heat treated coupons of 1.4542 and for comparison X20Cr13 and X46Cr13 were kept in the artificial brine of the Northern German Basin at T=60 °C. Ambient pressure as well as p=100 bar for 700 h - 8000 h in water saturated supercritical CO2 and CO2-saturated synthetic aquifer Environment was applied. Fatigue tests were performed via push-pull tests with a series of 30 specimens from 150 MPa to 500 MPa (sinusoidal dynamic test loads, R=-1; resonant frequency ~ 30 Hz). FeCO3 and FeOOH are corrosion products also after dynamic corrosion tests. Martensitic microstructure offers good corrosion resistance in geothermal environment. The S-N-curve showing no typical fatigue strength and very steep slopes of possible fatigue strength for finite life. Possible influencing artefacts, such as Al-inclusions could not be correlated to early rupture despite specimens containing inclusions at the fracture surface and cross section reached lower number of cycles. Applied potential proofed to enhance fatigue life tremendously. KW - High Alloyed Steel KW - Pitting KW - Corrosion Fatigue KW - Corrosion KW - Endurance Limit PY - 2019 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-503765 DO - https://doi.org/10.20319/mijst.2019.51.138158 SN - 2454-5880 VL - 5 IS - 1 SP - 138 EP - 158 PB - Global Research and Development Services Publishing CY - Rajasthan, India AN - OPUS4-50376 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Pfennig, A. A1 - Kranzmann, Axel T1 - Effect of CO2, atmosphere and pressure on the stability of C35CrMo17 stainless steel in laboratory CCS-environment N2 - During carbon sequestration the CO2-induced corrosion of injection pipe steels is a relevant safety issue when emission gasses are compressed into deep geological layers. The reliability of the high alloyed steel X35CrMo17 suitable as injection pipe for the geological onshore CCS-site (Carbon Capture and Storage) in the Northern German Basin, is demonstrated in laboratory experiments in equivalent corrosive environment (T = 60 °CC, p = 1–100 bar, aquifer water, CO2-flow rate of 9 L/h, 700–8000 h exposure time). Corrosion kinetics and microstructure were characterized and compared to other potential injection pipe steels (42CrMo4, X46Cr13, X20Cr13 and X5CrNiCuNb16-4). T2 - 14th Greenhouse Gas Control Technologies Conference CY - Melbourne, Australia DA - 21.10.2018 KW - Steel KW - Supercritical CO2 KW - Pipeline KW - Corrosion KW - CO2-storage PY - 2019 SP - 1 EP - 9 PB - Elsevier Ltd. AN - OPUS4-50382 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Pfennig, A. A1 - Wolf, M. A1 - Kranzmann, Axel T1 - The role of surface texture on the corrosion fatigue behavior of high alloyed stainless steel exposed to saline aquifer water environment N2 - Corrosion fatigue specimen with different surfaces (technical surfaces after machining and polished surfaces) of high alloyed martensitic stainless steel X46Cr13 (1.4043) and duplex stai nless steel X2CrNiMoN22 3 2 (1.4462) were compared at load amplitudes from 175 MPa to 325 MPa in the geothermal brine of the N orthern German Basin at 98 °C. Surface corrosion layers and pits reveal carbonate corrosion products on the surface such as FeCO 3 and FeOOH as the main precipitation phases with no dependence on the original surface roughness . At high stress amplitudes above 275 MPa technical surfaces (P50% at σa 300 MPa=5 × 10 5 ) resulted in more cycles to failure than polished (P50% at σa 300 MPa=1.5 × 10 5 ). The greater slope coefficient for technical surfaces k = 19.006 compared to polished surfaces k =8.78 demonstrate s earlier failure at given stress amplitude σa . KW - Corrosion KW - CCS KW - Carbon storage KW - Aquifer KW - Heat treatment PY - 2019 DO - https://doi.org/10.17706/ijmse SN - 2315-4527 VL - 7 IS - 2 SP - 26 EP - 33 PB - IAP - International Academy Publishing CY - San Bernardino, CA AN - OPUS4-50365 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Nolze, Gert A1 - Heide, K. T1 - Roaldite in the iron-meteorite São Julião de Moreira N2 - Roaldite – Fe4N – has been identified in the São Julião de Moreira iron meteorite using electron backscatter diffraction (EBSD) and simultaneously acquired energy-dispersive x-ray spectroscopy (EDS). Mean-periodic-number images derived from raw EBSD patterns confirm this phase by an even higher spatial resolution compared to EDS. Roaldite appears in the form of systematically and repetitively aligned plates. Despite the locally heavy plastic deformation, it is shown that the origin of the oriented precipitation of roaldite is linked to the orientation of the kamacite matrix. Roaldite can be considered to be precipitated from kamacite using an inverse Kurdjumov-Sachs (K-S) or Nishiyama-Wassermann (N-W) orientation relationship. A more accurate discrimination is impossible due to the accumulated shock deformation, which blurs the local reference orientation of kamacite. The habit plane of roaldite is found to be {112}R, which is most likely parallel to {120}K of kamacite. Some of the roaldite plates contain two orientation variants which repeatedly alternate. Their misorientation angle is about 12°. KW - Plastic deformation KW - Iron meteorite KW - Corrosion KW - Nitride KW - Orientation relationship PY - 2019 DO - https://doi.org/10.1016/j.chemer.2019.125538 VL - 79 IS - 4 SP - 125538 PB - Elsevier AN - OPUS4-50338 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Koerdt, Andrea A1 - An, Biwen Annie T1 - Investigation of methanogen-induced microbiologically influenced corrosion (Mi-MIC) using simulated marine environments under flowing conditions N2 - Microbiologically influenced corrosion (MIC) of iron is usually attributed to sulfate-reducing microorganisms (SRM) in oil and gas facilities. SRM act upon the metal by the re-activeness of hydrogen sulfide (HS-), and by withdrawal of the available electrons in electrical contact with the metal (EMIC). Methanogenic archaea (MA) can also cause MIC (Mi-MIC). Several MAs were identified to be corrosive by using elemental iron as the sole electron donor for methanogenesis, including Methanobacterium­-affliated IM1 and Methanococcus maripaludis Mic1c10. Currently, low corrosion rates were reported for MA, possibly due to the formation of siderite (4Fe + 5HCO3- + 5H+ ® 4FeCO3 + CH4 + 3H2O). Since MA do not produce HS-, withdrawal of electrons may be their main corrosive mechanism; however, mechanistic details and kinetics of the overall process are poorly understood. To investigate the corrosion potential of MA, we studied the EMIC methanogenic strains (IM1 and Mic1c10) individually or part of a syntrophic co-culture with SRM. Corrosion studies were conducted using an in-house developed flow-through system to simulate fluctuating environmental conditions. Results indicate that the rates of iron corrosion by MA (up to 0.4 mm/yr) are higher to that caused by the marine SRM Desulfovibrio alaskensis (0.15 mm/yr) and the co-culture (0.1 mm/yr). Scanning electron microscopy (SEM) images of the metal incubated with MA showed severe pitting corrosion. Genomic analysis of the EMIC MA was conducted to provide an insight on the possible cellular mechanisms that could be involved. Furthermore, low concentrations of MA-targeting biocides will be applied to EMIC MA in static and flow conditions to gain insights for possible mitigation strategies. Such knowledge and deeper understanding also from an electrokinetic point of view may not only provide further models in microbial electrophysiology, but also contribute to mitigation strategies in MIC. T2 - 7th International Symposium on Applied Microbiology and Molecular Biology in Oil Systems CY - Halifax, Canada DA - 18.06.2019 KW - MIC KW - Microbiologically influenced corrosion KW - Methanogens KW - SRB KW - Corrosion KW - Metalls PY - 2019 AN - OPUS4-48392 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Koerdt, Andrea T1 - Investigation of methanogen-induced microbiologically influenced corrosion (Mi-MIC) using simulated marine environments under flowing conditions N2 - Microbiologically influenced corrosion (MIC) of iron is usually attributed to sulfate-reducing microorganisms (SRM) in offshore industries, such as the oil and gas pipelines, due to the high concentrations of sulfate in the seawater. SRM act upon the metal by the reactiveness of hydrogen sulfide (HS-), and by withdrawal of the available electrons (Fe --> Fe2+ + 2e-; E° = -0.47 V) in electrical contact with the metal (EMIC). However, methanogenic archaea can also cause MIC. Because they do not produce HS-, withdrawal of electrons may be their main corrosive mechanism; however, mechanistic details and kinetics of the overall process are poorly understood. To investigate the corrosion potential of methanogens, we studied the EMIC methanogenic strains isolated from marine sediments (Methanobacterium-affiliated strain IM1) and crude oil tanks (Methanococcus maripaludis Mic1c10), in an in-house developed flow-through cell to simulate a fluctuating environment. A co-culture of M. maripaludis and D. alaskensis was also established to study the effect of syntrophic growth on metal corrosion that may occur in industrial pipelines. Results indicate that the rates of iron corrosion due to coupled methanogenesis (up to 0.4 mm/yr) are higher to that caused by the marine SRM Desulfovibrio alaskensis (0.15 mm/yr). Surface analyses of the metal showed severe pitting with high methane production. Genomic analysis of the EMIC methanogen M. maripaludis Mic1c10 will provide an insight on the mechanisms of MIC. Such knowledge and deeper understanding also from an electrokinetic point of view may not only provide further models in microbial electrophysiology, but also contribute to mitigation strategies in MIC. T2 - VAAM- Annual Conference 2019 of the Association for General and Applied Microbiology CY - Mainz, Germany DA - 17.03.2019 KW - HI-Tension KW - MIC KW - Methanogens KW - Corrosion KW - Sulfate reducing bacteria PY - 2019 AN - OPUS4-47739 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Koerdt, Andrea T1 - Investigation of methanogen-induced microbiologically influenced corrosion (Mi-MIC) using simulated marine environments under flowing conditions N2 - Microbiologically influenced corrosion (MIC) of iron is usually attributed to sulfate-reducing microorganisms (SRM) in offshore industries, such as the oil and gas pipelines, due to the high concentrations of sulfate in the seawater. SRM act upon the metal by the reactiveness of hydrogen sulfide (HS-), and by withdrawal of the available electrons (Fe --> Fe2+ + 2e-; E° = -0.47 V) in electrical contact with the metal (EMIC). However, methanogenic archaea can also cause MIC. Because they do not produce HS-, withdrawal of electrons may be their main corrosive mechanism; however, mechanistic details and kinetics of the overall process are poorly understood. To investigate the corrosion potential of methanogens, we studied the EMIC methanogenic strains isolated from marine sediments (Methanobacterium-affiliated strain IM1) and crude oil tanks (Methanococcus maripaludis Mic1c10), in an in-house developed flow-through cell to simulate a fluctuating environment. A co-culture of M. maripaludis and D. alaskensis was also established to study the effect of syntrophic growth on metal corrosion that may occur in industrial pipelines. Results indicate that the rates of iron corrosion due to coupled methanogenesis (up to 0.4 mm/yr) are higher to that caused by the marine SRM Desulfovibrio alaskensis (0.15 mm/yr). Surface analyses of the metal showed severe pitting with high methane production. Genomic analysis of the EMIC methanogen M. maripaludis Mic1c10 will provide an insight on the mechanisms of MIC. Such knowledge and deeper understanding also from an electrokinetic point of view may not only provide further models in microbial electrophysiology, but also contribute to mitigation strategies in MIC.zeige weniger T2 - Dechema CY - Berlin, Germany DA - 09.04.2019 KW - Corrosion KW - Corrosion products KW - Methanogens KW - Sulfate reducing bacteria KW - Flow-system KW - Environmental simulation PY - 2019 AN - OPUS4-47853 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Koerdt, Andrea T1 - Investigation of methanogen-induced microbiologically influenced corrosion (Mi-MIC) using simulated marine environments under flowing conditions N2 - Microbially influenced corrosion (MIC) of iron is usually attributed to sulfate-reducing microorganisms (SRM) which act upon the metal by the reactiveness of hydrogen sulfide, and by withdrawal of the available electrons in electrical contact with the metal. Methanogenic archaea can also cause MIC by directly withdrawing electrons from the iron surface for methanogenesis. However, the mechanistic details and kinetics of the overall process are poorly understood. Precipitation of siderite, a by-product of methanogenesis, (4Fe + 5HCO3 + 5H+  4FeCO3 + CH4 + 3H2O) can lead to an insulating layer on the metal surface and lower the corrosion rate. Still, the extent of FeCO3 precipitation may be significantly influenced by environmental conditions such as pH and advective processes. T2 - Dechema CY - Frankfurt a. M., Germany DA - 13.05.2019 KW - MIC KW - Corrosion KW - Methanogens KW - Corrosion product PY - 2019 AN - OPUS4-47982 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Reinemann, Steffi A1 - Rosemann, P. A1 - Babutzka, Martin A1 - Lehmann, Jens A1 - Burkert, Andreas T1 - Influence of grinding parameters on the corrosion behavior of austenitic stainless steel N2 - Samples of the austenitic stainless steel grade X5CrNi18‐10 (1.4301, AISI 304) were ground industrially with various grinding parameters to study their influence on corrosion resistance. The ability of the mechanically ground surfaces to form a stable passive layer was evaluated by KorroPad test and a modified electrochemical potentiodynamic reactivation test based on a single loop (EPR‐SL). Furthermore, the surfaces were characterized by surface analytical methods. The main influence was determined regarding abrasive belt type. Surfaces mechanically ground with granulate abrasive belts constantly had a lower corrosion resistance than surfaces ground with single‐coated grain. The granulate abrasive belts generated more sensitized surface areas and left formations of welded sample material on the mechanically ground surfaces. A post‐treatment with a nonwoven abrasive proved to be an effective finishing process by which the surface defects and sensitized material got removed and the surfaces regained the expected corrosion resistance. KW - Abrasive belt KW - Austenitic stainless steel KW - Electrochemical potentiodynamic reactivation KW - Grinding KW - KorroPad KW - Surface KW - Corrosion PY - 2019 DO - https://doi.org/10.1002/maco.201910874 SN - 0947-5117 SN - 1521-4176 VL - 70 IS - 10 SP - 1776 EP - 1787 PB - Wiley-VCH Verlag CY - Weinheim AN - OPUS4-47871 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Stephan-Scherb, Christiane T1 - Unravelling high temperature oxidation phenomena by in situ x-ray techniques N2 - Unravelling high temperature oxidation phenomena by in situ x-ray techniques. A multi techqnique approach to study high temperature gas corrosion is presented. T2 - Gordon Research Conference on High Temperature Corrosion CY - New London, NH, USA DA - 20.07.2019 KW - Corrosion KW - High temperature KW - Diffraction KW - Spectroscopy PY - 2019 AN - OPUS4-48772 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Kranzmann, Axel T1 - Corrosion of VM12 SHC in Salt melt N2 - Alkali and alkaline earth chlorides are discussed as heat storage media and are characterized by their low price and high availability. Disadvantages are a high corrosion rate and formation of Cr6+ ions in the melt, as observed in various binary chlorine salt melts. In our work the system NaCl-KCl-MgCl2 is considered. The storage capacity in this salt system is between 2 and 3 MWh per 10 t salt, depending on composition, melting temperature and working temperature. At the same time the system offers a eutectic line, which allows a high variance of the composition and possibly different corrosion rates can be observed. Corrosion tests in melts were carried out and the corrosion layers investigated. The tests with chloride melts on 12% Cr steel show an inner corrosion zone of up to 40 µm depth after 96 hours. The corrosion mechanisms and potential solutions are discussed. T2 - EUROCORR 2019 CY - Sevilla, Spain DA - 09.09.2019 KW - Salt melt KW - Corrosion KW - VM12 SHC PY - 2019 AN - OPUS4-50759 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - de Oliveira Guilherme Buzanich, Ana T1 - The versatility of X-ray absorption spectroscopy (XAS) for exploring new materials in collaborative research N2 - With increasing demand and environmental concerns, researchers are exploring new materials that can perform as well or better than traditional materials while reducing environmental impact. X-ray absorption spectroscopy (XAS) enables unique atom-specific tool to probe the electronic structure of materials. The BAM plays a central role in this highly collaborative research. The BAMline, a real-life sample materials research beamline, at the Berlin Synchrotron BESSY-II, provides unique insights into materials’ electronic and chemical structure at different time and length scales. This enables real-time optimization of material properties and performance for various applications, such as energy storage and conversion, catalysis, and corrosion resistance. This talk provides an overview of the analytical methods and sample environments of the BAMline and addresses its potential for further advances in sustainable materials research. T2 - International symposium of radiation physics (ISRP-16) CY - Lisbon, Portugal DA - 01.09.2024 KW - XAS KW - Time-resolved studies KW - Operando KW - Corrosion KW - Electrochemistry PY - 2024 AN - OPUS4-60996 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Stephan-Scherb, Christiane T1 - Early stages of high temperature oxidation/sulfidation studied by synchrotron x-ray diffraction and spectroscopy N2 - Ferritic high temperature alloys are widely used as boiler tube and heat exchanger materials in coal, biomass and co-fired power plants. All technologies have in common that the applied materials are exposed to different temperatures, process pressures and reactive atmospheres that lead to a change of the material properties and a further degradation of the material. Material changes caused by aging in highly corrosive and toxic gases such as SO2 are mainly studied ex situ after the reaction is finished. The solid material is deposited in the atmosphere for a certain period of time, and material changes are then examined by various microscopic techniques such as optical microscopy (OM), electron microprobe analysis (EMPA), scanning electron microscopy (SEM and TEM) and X-ray diffraction (XRD). Nevertheless, extensive efforts were made to study material changes of high temperature alloys under oxidizing and reducing atmospheres by environmental scanning electron microscopy or in situ TEM techniques However, the possibilities of microscopic in situ techniques are very limited for the use of highly corrosive and toxic gases such as SO2. Since Sulfur induced corrosion at temperatures relevant for coal and biomass fired power plants, which is causing breakaway oxidation and sulfide precipitation at grain boundaries, is still of scientific interest, the current work focuses on the effect of SO2 in an initial stage of corrosion of ferritic alloys. For the analysis of early stages of combined oxidation and sulphidation processes of Fe-Cr model alloys the usage of a light furnace to conduct a rapid reactive annealing experiment is feasible. Previous studies presented distinct results of the influence of chromium on early high temperature corrosion by SO2 by this technique and subsequent classical metallographic analyses. However, it is still not possible to trace the corrosion mechanism in real time by conducting single aging experiments. The current work introduces two different approaches to study the initial stages of high temperature oxidation processes by applying above state of the art X-ray diffraction and spectroscopy methods. One part focuses on the real time observation of the formation of corrosion products such as oxides and sulfides by energy dispersive X-ray diffraction (EDXRD). The potential of this technique to study crystallization and growth processes of thin films in a reactive environment in real time was previously shown for different compound semiconductors. This approach was now applied to follow oxidation and sulphidation processes of ferritic model alloys in SO2 and SO2/H2O environments. The diffraction signals of the X-rays were detected during the corrosion process and the peak area and positions were analyzed as a function of time. This procedure enables monitoring external oxide growth and material loss in real time in an early stage of corrosion. The other part of the current work presents the possibilities of X-ray absorption near edge structure spectroscopy (XANES) to characterize oxide scales and their growth mechanisms. Precise phase identification and quantification of corrosion products in a multi-phase oxide/sulfide scale is a pre-requisite to understand diffusion paths of metal ions and gas components. It is a challenging task to distinguish structurally similar reaction products such as Fe3O4 and FeCr2O4 especially in thin films with texture effects by diffraction. To illustrate for example Cr-out diffusion of an alloy throughout an inner and external oxide scale the differentiation of Fe3O4 and FeCr2O4 is indispensable. XANES uses the photoionization effect at the metal absorption edge in an aging product and accesses by this structural and chemical information. The current work uses XANES at the Fe-K and Cr-K absorption edge to identify various aging products grown as thin layers on alloys after short time aging experiments. A reaction chamber for combining high temperature oxidation experiments with surface sensitive X-ray absorption near edge structure spectroscopy will be introduced and first results of XANES on scales at high temperatures will be presented. T2 - ISHOC 2018 CY - Matsue, Japan DA - 22.10.2018 KW - Corrosion KW - Sulfidation KW - In situ KW - Diffraction KW - XANES PY - 2018 AN - OPUS4-47278 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - de Oliveira Guilherme Buzanich, Ana T1 - The versatility of X-ray absorption spectroscopy (XAS) for exploring new materials in collaborative research N2 - From Physics Engineer at FCUL in Lisbon to senior scientist at the Federal Institute for Materials Research and Testing (BAM) in Berlin, Germany. In this seminar, a personal journey using X-rays as a tool to probe different types of materials will be given. Examples of applications relevant to our society demonstrate how versatile and useful X-rays are T2 - Forschungsseminar an der FCUL (Univesity of Lisbon) CY - Online meeting DA - 25.10.2024 KW - XAS KW - Time-resolved studies KW - Operando KW - Corrosion KW - Electrochemistry PY - 2024 AN - OPUS4-61597 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Sobol, Oded A1 - Straub, F. A1 - Wirth, Thomas A1 - Holzlechner, G. A1 - Böllinghaus, Thomas A1 - Unger, Wolfgang T1 - Real Time Imaging of Deuterium in a Duplex Stainless Steel Microstructure by Time-of-Flight SIMS N2 - For more than one century, hydrogen assisted degradation of metallic microstructures has been identified as origin for severe technical component failures but the mechanisms behind have not yet been completely understood so far. Any in-situ observation of hydrogen transport phenomena in microstructures will provide more details for further elucidation of these degradation mechanisms. A novel experiment is presented which is designed to elucidate the permeation behaviour of deuterium in a microstructure of duplex stainless steel (DSS). A hydrogen permeation cell within a TOF-SIMS instrument enables electrochemical charging with deuterium through the inner surface of the cell made from DSS. The outer surface of the DSS permeation cell exposed to the vacuum has been imaged by TOF-SIMS vs. increasing time of charging with subsequent chemometric treatment of image data. This in-situ experiment showed evidently that deuterium is permeating much faster through the ferrite phase than through the austenite phase. Moreover, a direct proof for deuterium enrichment at the austenite-ferrite interface has been found. KW - Characterization and analytical techniques KW - Corrosion KW - Imaging technique KW - Mass spectrometry PY - 2016 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-353872 UR - http://www.nature.com/articles/srep19929 DO - https://doi.org/10.1038/srep19929 SN - 2045-2322 VL - 6 IS - 19929 SP - 1 EP - 7 PB - nature publishing group CY - London, United Kingdom AN - OPUS4-35387 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Nolze, Gert A1 - Saliwan Neumann, Romeo A1 - Buchheim, Michaela T1 - Microstructure investigations of iron meteorites by EBSD and EDS analyses N2 - Meteorites are a unique and inspiring material for microstructural studies because if their very specific genesis. Iron meteorites have been formed under unimaginable cooling rates of a few ten Kelvins per million years so that the observable transformation of the formerly huge Fe-Ni single crystals of taenite occurred under nearly-equilibrium conditions. Octahedrites (meteorites having a Ni content between 6...15%) are characterized by ribbons of the low-temperature Fe-Ni phase kamacite separated by rims of residual taenite. This very specific feature is known as Widmanstaetten structure and has been investigated by synchrotron radiation in order to cover a higher volume fraction for a statistically relevant description of orientation relationships. However, plessite – a microstructure mainly consisting of the same phases – reflects the orientation relationship between kamacite and taenite as well. For their characterization, a scanning electron microscope is very suitable in order to investigate crystal orientations or identify phases. Despite the apparently ideal formation circumstances of iron meteorites, Ni concentration profiles prove non-equilibrium conditions. Combined EDS (energy dispersive spectroscopy) and EBSD (electron backscatter diffraction) measurements at a selected plessitic region of the Cape York iron shows that a correlation exists between Ni-concentration and the locally detected orientation relationship. T2 - 15th European Microscopy Congress CY - Manchester, UK DA - 16.09.2012 KW - Phase identification KW - Corrosion KW - Chloride KW - Dermbach PY - 2012 SP - 90 AN - OPUS4-37775 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - An, Biwen Annie T1 - Investigating the effects of biocides and corrosion inhibitors on corrosive methanogens N2 - Microbiologically influenced corrosion (MIC) is the deterioration of metals due to the metabolic activities of microorganisms. Microorganisms can take electrons directly from the metal surface (EMIC) thereby causing corrosion. Well known culprits of EMIC are: sulfate-reducing bacteria (SRB), acetogens and methanogens. Our aims - Develop a novel flow system to study MIC by methanogens to mimic industrial Environments - Investigate the inhibitory concentrations of biocides targeting SRB on corrosive methanogenic strains - Investigate the inhibitory effects of corrosion inhibitors on methanogens - Compare the inhibitory concentrations to SRB T2 - BAM meeting CY - BAM, Berlin, Germany DA - 06.06.2018 KW - MIC projekt KW - Mikrobiell beeinflusste Korrosion KW - Microbiologically influenced corrosion KW - Korrosion KW - Corrosion KW - Material degradation KW - Biocide PY - 2018 AN - OPUS4-46010 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Koerdt, Andrea T1 - Investigating the effects of biocides and corrosion inhibitors on corrosive methanogens N2 - Microbiologically influenced corrosion (MIC) is the deterioration of metals due to the metabolic activities of microorganisms. Microorganisms can take electrons directly from the metal surface (EMIC) thereby causing corrosion. Well known culprits of EMIC are: sulfate-reducing bacteria (SRB), acetogens and methanogens. T2 - AMiCI WG2 workshop Berlin CY - Berlin, Germany DA - 7.7.2018 KW - Corrosion KW - Biocides KW - Methanogens PY - 2018 AN - OPUS4-45734 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Nikoonasab, Ali T1 - Electrochemical study of steel reinforcement in the synthetic pore solution of alkali-activated binders: Pore solution composition N2 - It is well known that cement manufacture, including CaCO3 calcination and clinker formation, is associated with substantial energy consumption and significant greenhouse gas emissions. Alkali-activated binders (AAB) and concretes made from them can significantly contribute to reducing CO2 emissions caused by the construction industry. However, to what extent and for how long concretes made from AAB can protect the steel in reinforced concrete components from corrosion is still unclear. Unlike PC-based binders, AABs are made by reacting alkaline solutions with solid precursors such as fly ash and ground granulated blast furnace slag (GGBFS). Therefore, steel reinforcement corrosion mechanisms in AAMs differ from PC-based binders. The present study aims to evaluate the corrosion behavior of steel rebar in alkali-activated materials (AAMs) synthetic pore solution with different chemical concentrations representing different GGBFS and Flay Ash based binders by performing electrochemical tests to measure the corrosion rate and corrosion potential of steel rebar. This information can be used to improve the design of AAMs in order to ensure a longer service life for these materials. T2 - Eurocorr2023 CY - Brussels, Belgium DA - 27.08.2023 KW - GGBFS KW - AAM KW - Sulfide KW - Pore solution composition KW - Redox potential KW - Corrosion PY - 2023 AN - OPUS4-59090 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER -