TY - JOUR A1 - Rösler, Alexander A1 - Weidner, Steffen A1 - Klamroth, Tillmann A1 - Müller, Axel HE A1 - Schlaad, Helmut T1 - Kinetics of anionic polymerization of β‐myrcene in hydrocarbon solvents N2 - AbstractThe kinetics of anionic polymerization of β‐myrcene initiated by sec‐butyllithium were examined in saturated and unsaturated hydrocarbon solvents, i.e. cyclohexane, cyclohexene, 4‐vinylcyclohexene and dl‐limonene. Polymerizations usually proceeded in a living manner, i.e. in the absence of termination and chain transfer reactions, in all solvents, to produce well‐defined polymyrcenes with high content (85%) of cis‐1,4 units. However, polymyrcenyllithium chains exhibited limited long‐term stability in 4‐vinylcyclohexene solution, most probably due to chain transfer to solvent. Reaction orders with respect to the concentration of active chains were found to be one‐quarter in cyclohexane increasing to one‐half in unsaturated solvents, indicating that the polymyrcenyllithium chains are present as tetrameric or dimeric associates, respectively. Apparent activation energies were found to be 81 kJ mol−1 in cyclohexane and 77 kJ mol−1 in dl‐limonene solution, which are close to the values obtained by quantum chemical calculations. © 2025 The Author(s). Polymer International published by John Wiley & Sons Ltd on behalf of Society of Chemical Industry. KW - Myrcene KW - Anionic polymerization KW - MALDI TOF MS PY - 2025 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-649039 DO - https://doi.org/10.1002/pi.6772 SN - 0959-8103 SP - 1 EP - 8 PB - Wiley AN - OPUS4-64903 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Weidner, Steffen A1 - Kühn, Gerhard A1 - Decker, Renate A1 - Roessner, D. A1 - Friedrich, Jörg Florian T1 - Influence of Plasma Treatment on the Molar Mass of Poly(ethylene terephthalate) Investigated by Different Chromatographic and Spectroscopic Methods N2 - The influence of different types of low and atmospheric pressure plasma on poly(ethylene terephthalate) (PET) has been studied in terms of changes in molar mass and molar mass distribution. Apart from a variation of plasma gases (oxygen, helium) different types of plasma (microwave, radio frequency, corona discharge) were used for the plasma surface modification. The changes in molar mass and types of functional end groups of lower molar mass products were investigated by means of matrix-assisted laser desorption/ionization time of flight mass spectrometry (MALDI-TOFMS), whereas the high-molar mass fraction was analyzed by means of size-exclusion chromatography (SEC). The formation of crosslinked products during exposure to a helium plasma, which emits preponderately energy-rich and intense ultraviolet radiation, was proved by means of thermal field-flow fractionation (ThFFF). This method combined with a multiangle laser light scattering (MALLS) detector allows detection of weakly crosslinked polymers and microgels. © 1998 John Wiley & Sons, Inc. J Polym Sci A: Polym Chem 36: 1639-1648, 1998 KW - Poly(ethylene terephthalate) KW - PET KW - Plasma PY - 1998 UR - http://www3.interscience.wiley.com/cgi-bin/abstract/36482/ABSTRACT DO - https://doi.org/10.1002/(SICI)1099-0518(19980730)36:10<1639::AID-POLA17>3.0.CO;2-H SN - 0360-6376 SN - 0887-624X VL - 36 IS - 10 SP - 1639 EP - 1648 PB - Wiley CY - Hoboken, NJ AN - OPUS4-6989 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Czichocki, G. A1 - Fiedler, H. A1 - Haage, K. A1 - Much, Helmut A1 - Weidner, Steffen T1 - Characterization of alkyl polyglycosides by both reversed-phase and normal-phase modes of high-performance liquid chromatography N2 - Alkyl polyglycosides today represent the most important sugar surfactant. Nonionic sugar surfactants produced via different synthetic routes are mixtures of alkyl homologues, oligomers, anomers and isomers. Alkyl homologues and oligomers of alkyl mono- and diglucosides were separated by reversed-phase high-performance liquid chromatography (HPLC) with methanol–water as the mobile phase using a gradient elution. The gradient was optimized in respect to a simultaneous separation of alkyl glycosides according to their alkyl chain length and alkyl polyoxyethylene glucosides with regard to their length of the polyoxyethylene spacer. The separation of alkyl glycosides into ?- and ?-anomers was carried out by normal-phase HPLC with isooctane–ethyl acetate (60:40, v/v)–2-propanol in the gradient mode. Light scattering detection was used. Matrix-assisted laser desorption ionization time-of-flight mass spectra of alkyl glucosides and dodecyl glucosides with oxyethylene spacer groups are presented. PY - 2002 DO - https://doi.org/10.1016/S0021-9673(01)01459-5 SN - 0021-9673 VL - 943 IS - 2 SP - 241 EP - 250 PB - Elsevier CY - Amsterdam AN - OPUS4-11099 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Braun, Ulrike A1 - Wachtendorf, Volker A1 - Geburtig, Anja A1 - Bahr, Horst A1 - Schartel, Bernhard T1 - Weathering resistance of halogen-free flame retardance in thermoplastics N2 - The influence of weathering on the fire retardancy of polymers is investigated by means of a cone calorimeter test, before and after artificial weathering. The surface degradation was monitored using different techniques (ATR–FTIR, microscopy, colour measurement). Different kinds of polymeric materials were chosen, all as they are used in practice: polycarbonate (PC) blends, polyamide (PA) and polypropylene (PP) flame-retarded with arylphosphate, melamine cyanurate (MC) and intumescent formulation based on ammonium polyphosphate (APP), respectively. All samples show material degradation at the surface due to weathering. No significant weathering influence occurs on the flame retardancy when it is a bulk property, as was observed for aryl phosphates in PC blends and MC in PA. When the fire retardancy is dominated by a surface mechanism, dependence on the duration of weathering is detected: for intumescent formulations based on ammonium APP in PP, a worsening in the formation of the intumescent network was observed. KW - Fire retardancy KW - Weathering resistance KW - Degradation KW - Intumescence KW - Cone calorimeter PY - 2010 DO - https://doi.org/10.1016/j.polymdegradstab.2010.08.020 SN - 0141-3910 SN - 1873-2321 VL - 95 IS - 12 SP - 2421 EP - 2429 PB - Applied Science Publ. CY - London AN - OPUS4-22612 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Geburtig, Anja A1 - Wachtendorf, Volker A1 - Trubiroha, Peter T1 - The Principle of Reciprocity and its Limits T2 - 3rd European Weathering Symposium CY - Krakow, Poland DA - 2007-09-12 KW - Spectral sensitivity KW - Weathering KW - UV KW - Action spectra KW - Activation spectra KW - Stabilizer KW - Spektrale Empfindlichkeit KW - Bewitterung KW - Aktivierungsspektrum KW - Wirkungsspektrum KW - Stabilisator PY - 2007 SN - 978-3-9810472-3-3 VL - 8 SP - 243 EP - 258 CY - Pfinztal AN - OPUS4-15925 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Geburtig, Anja A1 - Goedecke, Thomas A1 - Wachtendorf, Volker T1 - Combined impact of ultraviolet and chemical fluids on high-density polyethylene packaging material N2 - To investigate the ageing behaviour of filled plastic containers outdoors, square cuts of the wall of two high-density polyethylene (HDPE) types were exposed to ultraviolet (UV) radiation at their front side and to specific liquid chemicals (de-ionized water, surfactant or White Spirit) at their back. The UV radiant exposure at the front side was 80 MJ/m². To compare the actions of the different exposures, separate dark backside fluid exposures were performed, in parallel. Besides, UV weathering was carried out until a UV radiant exposure of 325 MJ/m², being roughly comparable to outdoor exposure of one year in Northern Australia. An unpigmented HDPE included in the investigation gave no sufficient protection for the White Spirit. In addition, it showed clear degradation after several of these exposures. In combination with the White Spirit, an increase of carbonyl bonds was measured, presumably assignable to degradation products of the White Spirit. For a pigmented HDPE material, with the implemented combined exposures, no relevant damage was observed, within applied the exposure period. KW - Weathering KW - UV KW - HDPE KW - Packaging PY - 2012 DO - https://doi.org/10.1002/pts.959 SN - 0894-3214 VL - 25 IS - 1 SP - 53 EP - 61 PB - Wiley CY - Chichester, UK AN - OPUS4-25417 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Geburtig, Anja A1 - Wachtendorf, Volker A1 - Trubiroha, Peter T1 - Referenzmaterialien für Bewitterungsprüfungen T2 - 32. Jahrestagung der GUS, Gesellschaft für Umweltsimulation CY - Pfinztal bei Karlsruhe, Deutschland DA - 2003-03-26 KW - Referenzmaterialien KW - Bewitterung PY - 2003 SN - 3-9808382-1-8 SP - 61 EP - 72 PB - GUS CY - Pfinztal (Berghausen) AN - OPUS4-3360 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Anik, Yavuz A1 - Geburtig, Anja A1 - Sturm, Heinz A1 - Meyer-Plath, Asmus ED - Reichert, T. T1 - CarboLifeCycle -weathering-induced degradation of nanoparticle-functionalised composites N2 - A new research project 'CarboLifeCycle', funded by the German Federal Ministry of Education and Research (BMBF), investigates various nanoparticle release scenarios for carbon nanotube-containing polymer composites. The studied weathering concepts and conditions will be described. T2 - 5th European weathering symposium - Natural and artificial ageing of polymers CY - Lisbon, Portugal DA - 21.09.2011 KW - CNT KW - Nanoparticle KW - Weathering KW - Degradation PY - 2011 SN - 978-3-9813136-2-8 N1 - Serientitel: CEEES Publication – Series title: CEEES Publication IS - 15 SP - 125 EP - 135 PB - GUS (Gesellschaft für Umweltsimulation) CY - Pfinztal AN - OPUS4-24503 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Geburtig, Anja A1 - Wachtendorf, Volker A1 - Trubiroha, Peter T1 - Accelerated weathering test for plastics and coatings that are exposed to acidic precipitation N2 - Due to the occurrence of acidic precipitation, and due to the fact that polymers and stabilizers may be sensititve to acids, it is important to have a laboratory test that combines weathering exposure with acidic exposure. The loss of stabilization caused by an acid damage of stabilizing system gets evident only over the weathering progress. For solid samples, for wich mostly the surface properties are relevant, the "Acid Dew and Fog Test" (ADF test) was established. For woven or tufted materials, the "Acid Rain Test" (AR test) was developed. The proposed weathering tests aim at plastics as well as at coatings. T2 - 7th International Symposium on Weatherability (7th ISW) CY - Kanagawa, Japan DA - 2008-10-23 KW - Acid rain KW - ADF KW - Acid Dew and Fog test KW - Artificial Weathering test PY - 2009 SN - 1346-0633 VL - 21 IS - 2 SP - 69 EP - 73 PB - Materiaru-Raifu-Gakkai CY - Tokyo AN - OPUS4-18270 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Wachtendorf, Volker A1 - Geburtig, Anja A1 - Trubiroha, Peter ED - Jonathan W. Martin, ED - Rose A. Ryntz, ED - J. Chin, ED - Ray A. Dickie, T1 - Chemiluminescence detection: Principles, chances and limitations for the shortening of weathering tests T2 - 4th International Symposium on Service Life Prediction CY - Key Largo, FL, USA DA - 2006-12-03 KW - Chemiluminescence KW - Weathering KW - Quantum efficiency KW - Accelerated test KW - Automotive coating KW - PE Chemilumineszenz KW - Bewitterung KW - Quantenausbeute KW - Beschleunigter Test KW - Automobillacke PY - 2008 SN - 978-0-387-84875-4 SP - 309 EP - 326 PB - Springer AN - OPUS4-18245 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Trubiroha, Peter A1 - Wachtendorf, Volker A1 - Geburtig, Anja ED - Ziegahn, K.-F. T1 - Beispiele für die Nutzung des Energietransports durch langwellige (thermische) Strahlung T2 - 35. Jahrestagung der GUS 2006 - Umwelteinflüsse erfassen, simulieren, bewerten CY - Pfinztal, Deutschland DA - 2006-03-22 PY - 2006 SN - 3-9810472-0-6 SP - 205 EP - 214 PB - DWS Werbeagentur und Verlag GmbH CY - Pfinztal AN - OPUS4-21347 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Geburtig, Anja A1 - Wachtendorf, Volker A1 - Trubiroha, Peter T1 - Improved Evaluation of Activation Spectra Determined by the Filter Technique T2 - 3rd European Weathering Symposium CY - Krakow, Poland DA - 2007-09-12 KW - Spectral sensitivity KW - Weathering KW - UV KW - Action spectra KW - Activation spectra KW - Stabilizer KW - Spektrale Empfindlichkeit KW - Bewitterung KW - Aktivierungsspektrum KW - Wirkungsspektrum KW - Stabilisator PY - 2007 SN - 978-3-9810472-3-3 VL - 8 SP - 349 EP - 358 CY - Pfinztal AN - OPUS4-15924 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER -