TY - CONF A1 - Brandić Lipińska, M. A1 - Davenport, R. A1 - Imhof, A. B. A1 - Waclavicek, R. A1 - Fateri, M. A1 - Meyer, Lena A1 - Gines-Palomares, J. C. A1 - Zocca, Andrea A1 - Makaya, A. A1 - Günster, Jens T1 - PAVER - Contextualizing laser sintering within a lunar technology roadmap N2 - The Global Exploration Strategy of the International Space Exploration Coordination Group (ISECG) describes a timeframe of 2020 and beyond with the ultimate aim to establish a human presence on Mars towards the 2040ies. The next steps lie on the Moon with a focus on the coming 10 years. Early lunar surface missions will establish a capability in support of lunar science and prepare and test mission operations for subsequent human exploration of Mars and long-duration human activities on the Moon. Given the extreme costs involved in the shipping of material from Earth, a prerequisite for future human exploration is the manufacturing of elements directly on the Moon’s surface. Unlike the equipment, which at the beginning will have to be brought from Earth, raw materials and energy could be available following the concept of In-Situ Resource Utilization. The ESA OSIP PAVING THE ROAD (PAVER) study investigates the use of a laser to sinter regolith into paving elements for use as roadways and launch pads thus mitigating dust issues for transport and exploration vehicles. The ESA-funded study examines the potential of using a laser (12 kW CO2 laser with spot beam up to 100 mm) for layer sintering of lunar and martian regolith powders to manufacture larger 3D elements and provide know-how for the automatic manufacture of paving elements in the lunar environment. The project contributes to the first step toward the establishment of a lunar base and will lead to the construction of equipment capable of paving areas and manufacturing 3D structures. PAVER project sets the starting point for an examination of the larger context of lunar exploration. Mission scenarios will look at different phases of lunar exploration: Robotic Lunar Exploration, Survivability, Sustainability, and Operational Phase. A proposed Technology Roadmap investigates the mission scenario and analyses how, and to which extent, laser melting/sintering will play a role in the various phases of exploration. The paper contextualizes laser sintering within selected mission scenarios and discusses the different kinds of infrastructure that can be produced at each phase of the mission. The outcome of the study includes the detailing of the TRL steps in the project and an outline of a timeline for the different elements. Covered aspects include terrain modelling such as operation pads, roadways, or towers, non-pressurized building structures to protect machinery, and habitat envelopes, to protect and shield humans against dust, micrometeoroids, and radiation. T2 - 73rd International Astronautical Congress (IAC) CY - Paris, France DA - 18.09.2022 KW - Additive manufacturing KW - Solar sintering KW - ISRU KW - Infrastructure KW - Lunar habitat KW - Paving PY - 2022 SP - 1 EP - 9 AN - OPUS4-56519 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Günster, Jens A1 - Meyer, Lena T1 - Laser beam melting additive manufacturing at μ-gravity N2 - At the Workshop "Neutron and Synchrotron Monitoring in Aerospace Advanced Manufacturing" at the Institute of Materials Physics in Space, German Aerospace Center (DLR) in Cologne, we presented on the opportunities and our experiences of using a powder based additive manufacturing process for in-space manufacturing applications in microgravity. T2 - Workshop 'Neutron and Synchrotron Monitoring in Aerospace Advanced Manufacturing' CY - Cologne, Germany DA - 11.08.2022 KW - Additive manufacturing KW - In-space manufacturing KW - Microgravity KW - μ-gravity KW - Laser beam melting KW - Advanced manufacturing KW - Aerospace KW - Process monitoring PY - 2022 AN - OPUS4-56521 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Zocca, Andrea A1 - Schubert, Hendrik A1 - Günster, Jens T1 - Combination of layerwise slurry deposition and binder jetting (lsd-print) for the additive manufacturing of advanced ceramic materials N2 - Powder bed technologies are amongst the most successful Additive Manufacturing (AM) techniques. Powder bed fusion and binder jetting especially are leading AM technologies for metals and polymers, thanks to their high productivity and scalability. The application of these techniques to most ceramics has been difficult so far, because of the challenges related to the deposition of homogeneous powder layers when using fine powders. In this context, the “layerwise slurry deposition” (LSD) has been developed as a layer deposition method which enables the use of powder bed AM technologies also for advanced ceramic materials. The layerwise slurry deposition consists of the layer-by-layer deposition of a ceramic slurry by means of a doctor blade, in which the slurry is deposited and dried to achieve a highly packed powder layer. This offers high flexibility in the ceramic feedstock used, especially concerning material and particle size. The LSD technology can be combined with binder jetting to develop the so-called “LSDprint” process for the additive manufacturing of ceramics. The LSDprint technology combines the high-speed printing of binder jetting with the possibility of producing a variety of high-quality ceramics with properties comparable to those achieved by traditional processing. In this presentation, the LSD process will be introduced and several examples of application ranging from silicate to high-performance ceramics will be shown. Recent developments towards the scale-up and industrialization of this process will be discussed, alongside future perspectives for the multi-material additive manufacturing. T2 - Shaping 8 CY - Dübendorf, Switzerland DA - 14.09.2022 KW - Additive Manufacturing KW - 3D printing KW - Ceramics PY - 2022 AN - OPUS4-56523 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Brandić Lipińska, M. A1 - Davenport, R. A1 - Imhof, A. B. A1 - Waclavicek, R. A1 - Fateri, M. A1 - Meyer, Lena A1 - Gines-Palomares, J. C. A1 - Zocca, Andrea A1 - Makaya, A. A1 - Günster, Jens T1 - PAVER - Contextualizing laser sintering within a lunar technology roadmap N2 - The Global Exploration Strategy of the International Space Exploration Coordination Group (ISECG) describes a timeframe of 2020 and beyond with the ultimate aim to establish a human presence on Mars towards the 2040ies. The next steps lie on the Moon with a focus on the coming 10 years. Early lunar surface missions will establish a capability in support of lunar science and prepare and test mission operations for subsequent human exploration of Mars and long-duration human activities on the Moon. Given the extreme costs involved in the shipping of material from Earth, a prerequisite for future human exploration is the manufacturing of elements directly on the Moon’s surface. Unlike the equipment, which at the beginning will have to be brought from Earth, raw materials and energy could be available following the concept of In-Situ Resource Utilization. The ESA OSIP PAVING THE ROAD (PAVER) study investigates the use of a laser to sinter regolith into paving elements for use as roadways and launch pads thus mitigating dust issues for transport and exploration vehicles. The ESA-funded study examines the potential of using a laser (12 kW CO2 laser with spot beam up to 100 mm) for layer sintering of lunar and martian regolith powders to manufacture larger 3D elements and provide know-how for the automatic manufacture of paving elements in the lunar environment. The project contributes to the first step toward the establishment of a lunar base and will lead to the construction of equipment capable of paving areas and manufacturing 3D structures. PAVER project sets the starting point for an examination of the larger context of lunar exploration. Mission scenarios will look at different phases of lunar exploration: Robotic Lunar Exploration, Survivability, Sustainability, and Operational Phase. A proposed Technology Roadmap investigates the mission scenario and analyses how, and to which extent, laser melting/sintering will play a role in the various phases of exploration. The paper contextualizes laser sintering within selected mission scenarios and discusses the different kinds of infrastructure that can be produced at each phase of the mission. The outcome of the study includes the detailing of the TRL steps in the project and an outline of a timeline for the different elements. Covered aspects include terrain modelling such as operation pads, roadways, or towers, non-pressurized building structures to protect machinery, and habitat envelopes, to protect and shield humans against dust, micrometeoroids, and radiation. T2 - 73rd International Astronautical Congress (IAC) CY - Paris, France DA - 18.09.2022 KW - Additive manufacturing KW - ISRU KW - Infrastructure KW - Lunar habitat KW - Paving KW - Solar sintering PY - 2022 AN - OPUS4-56529 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Shakeel, Y. A1 - Soysal, M. A1 - Vitali, E. A1 - Ost, P. A1 - Aversa, R. A1 - Ávila Calderón, Luis Alexander A1 - Engstler, M. A1 - Fell, J. A1 - Fritzen, F. A1 - Hermmann, H.-G. A1 - Laadhar, A. A1 - Olbricht, Jürgen A1 - Pauly, C. A1 - Roland, M. A1 - Skrotzki, Birgit T1 - NFDI-MatWerk - Reference Datasets N2 - Within NFDI-MatWerk (“National Research Data Infrastructure for Material Sciences”/ “Nationale Forschungsdateninfrastruktur für Materialwissenschaften und Werkstofftechnik“), the Task Area Materials Data Infrastructure (TA-MDI) will provide tools and services to easily store, share, search, and analyze data and metadata. Such a digital materials environment will ensure data integrity, provenance, and authorship. The MatWerk consortium aims to develop specific solutions jointly with Participant Projects (PPs), which are scientific groups or institutes covering different domains, from theory and simulations to experiments. The Data Exploitation Methods group of the Karlsruhe Institute of Technology-Steinbuch Centre of Computing, as part of TA-MDI, is developing specific solutions in close collaboration with three PPs. PP07, together with the University of Stuttgart, aims at the image-based prediction of the material properties of stochastic microstructures using large-scale supercomputers. PP13, in cooperation with the University of Saarland, focuses on tomographic methods at various scales in materials research. PP18, together with the Federal Institute for Materials Research and Testing (“Bundesanstalt für Materialforschung und -prüfung”), aspires to define the criteria for materials reference datasets and usage analytics. The requirements and goals are comparable for each PP: their research outputs, which are scientific datasets, should conform to the FAIR (Findable, Accessible, Interoperable, Reusable) principles. We aim to shape them from a data management perspective making use of the FAIR Digital Object concept, including structured metadata and storage solutions. The results will be a blueprint which will act as a reference for future datasets. Even though the collaboration is in an early stage, the initial steps already show the added value of this approach. This research has been supported by the Federal Ministry of Education and Research (BMBF) – funding code M532701 / the Deutsche Forschungsgemeinschaft (DFG, German Research Foundation) - project number NFDI 38/1, project no. 460247524. T2 - HMC Conference 2022 CY - Online meeting DA - 05.10.2022 KW - NFDI KW - NFDI-MatWerk KW - Reference Data KW - FAIR KW - Creep PY - 2022 AN - OPUS4-56611 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Alig, I. A1 - Oehler, H. A1 - Brauch, Niels A1 - Thuy, Maximilian A1 - Niebergall, Ute A1 - Böhning, Martin T1 - Charakterisierung von Behälterwerkstoffen aus Polyethylen N2 - Das langsame Risswachstum (slow crack growth, SCG) sowie der umgebungsbedingte Spannungsriss (environmental stress cracking, ESC) sind relevante Schädigungsmechanismen für teilkristalline Werkstoffe auf Basis von Polyethylen hoher Dichte (PE-HD). Der Vortrag gibt einerseits einen Überblick über die grundlegenden Struktur-Eigenschafts-Beziehungen in diesem Kontext, andererseits werden auch verschiedene praxisorientierte Prüfverfahren vorgestellt. Letztere wurden in gemeinsamen Forschungsprojekten von BAM und LBF mit dem Schwerpunkt Gefahrgutbehälter bzw. Pflanzenschutzmittel vergleichend untersucht und durch weitergehende Analytik ergänzt. T2 - 16. Tagung des Arbeitskreises Polymeranalytik Webkonferenz, Fraunhofer LBF und FGK CY - Online meeting DA - 22.03.2022 KW - Polyethylen KW - Full Notch Creep Test KW - Environmental Stress Cracking KW - Spannungsriss PY - 2022 AN - OPUS4-54547 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Riechers, Birte A1 - Roed, L. A1 - Mehri, S. A1 - Ingebrigtsen, T. A1 - Hecksher, T. A1 - Dyre, J. A1 - Niss, K. T1 - Predicting nonlinear physical aging of glasses from equilibrium relaxation via the material time N2 - The noncrystalline glassy state of matter plays a role in virtually all fields of materials science and offers complementary properties to those of the crystalline counterpart. The caveat of the glassy state is that it is out of equilibrium and therefore exhibits physical aging, i.e., material properties change over time. For half a century, the physical aging of glasses has been known to be described well by the material-time concept, although the existence of a material time has never been directly validated. We do this here by successfully predicting the aging of the molecular glass 4-vinyl-1,3-dioxolan-2-one from its linear relaxation behavior. This establishes the defining property of the material time. Via the fluctuation-dissipation theorem, our results imply that physical aging can be predicted from thermal-equilibrium fluctuation data, which is confirmed by computer simulations of a binary liquid mixture. KW - Physical aging KW - Equilibrium relaxation KW - Glass PY - 2022 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-546015 DO - https://doi.org/10.1126/sciadv.abl9809 SN - 2375-2548 VL - 8 IS - 11 SP - 1 EP - 8 PB - American Association for the Advancement of Science CY - Washington, DC AN - OPUS4-54601 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Han, Ying A1 - Radners, J. A1 - von Hartrott, P. A1 - Skrotzki, Birgit T1 - Aluminium high temperature fatigue N2 - The studied aluminium alloy is EN AW-2618A (2618A). It is very widely used for exhaust gas turbo-charger compressor wheels. Due to long operating times, high cycle fatigue (HCF) and material aging under the influence of temperatures up to 230 °C is particularly relevant for the wheels. The wheels are typically milled from round wrought blanks. From such round blanks, different testpieces are extracted and a comprehensive series of HCF tests is conducted at room temperature. The tests investigate the materials fatigue performance in the T61 state for two load-ratios, namely R = -1 and R = 0.1. Additionally, two overaged material states are tested, accounting for the aging process the material undergoes during long operating times at high temperatures. The experimental results are evaluated and compared to each other. Furthermore, the design process of notched specimens is presented. With the notched specimens, it is aimed to quantify the notch sensitivity of the material. Relating thereto, two potential model parameters for the fatigue lifetime model are introduced. Finally, the extended research data management in this project is highlighted and its advantages for sustainable use in material science and engineering applications are shown. N2 - In diesem Projekt wird die Aluminiumlegierung EN AW-2618A (2618A) untersucht, welche sehr verbreitet in Verdichterrädern von Abgasturboladern zum Einsatz kommt. Hochzyklische Ermüdung und Werkstoffalterung bei Temperaturen von bis zu 230 °C ist bei Abgasturboladern aufgrund der langen Einsatzzeiten besonders relevant. Die Verdichterräder werden typischerweise aus geschmiedeten Rohlingen gefräst. Aus entsprechenden Rohlingen werden im Rahmen des Projekts eine Vielzahl von Proben mit unterschiedlichen Geometrien entnommen. Die Proben werden unter verschiedenen Prüfbedingungen in hochzyklischen Ermüdungsversuchen bei Raumtemperatur getestet. Zum einen wird das Ermüdungsverhalten des Werkstoffs im T61-Zustand für die zwei Belastungsverhältnisse R = -1 und R = 0,1 untersucht. Zum anderen werden zwei überalterte Materialzustände getestet. Damit soll dem Alterungsprozess Rechnung getragen werden, den das Material während langer Betriebszeiten bei hohen Temperaturen durchläuft. Die experimentellen Ergebnisse werden evaluiert und miteinander verglichen. Darüber hinaus wird der Entwurfsprozess von gekerbten Probengeometrien dokumentiert. Die gekerbten Proben sollen Aufschluss über die Kerbempfindlichkeit des Werkstoffs geben. In diesem Zusammenhang werden zwei mögliche Modellparameter für das zu entwickelnde Lebensdauermodell vorgestellt. Abschließend wird das erweiterte Forschungsdatenmanagement des Projekts beleuchtet und seine Vorteile für die nachhaltige Nutzung in materialwissenschaftlichen und ingenieurtechnischen Anwendungen aufgezeigt. T2 - FVV Frühjahrstagung 2022 CY - Würzburg, Germany DA - 31.03.2022 KW - EN AW-2618A KW - High cycle fatigue KW - Aluminium alloy PY - 2022 IS - FVV Publikationen Heft R602 SP - 617 EP - 634 PB - Forschungsvereinigung Verbrennungskraftmaschinen (FVV) CY - Frankfurt am Main AN - OPUS4-54622 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - THES A1 - Nielow, Dustin T1 - Einfluss fertigungsbedingter Imperfektionen auf die Schwingfestigkeit von FKV-Schalenstrukturen in Sandwichbauweise N2 - Rotorblätter von Windenergieanlagen (WEA) weisen häufig nach wenigen Jahren, lange vor dem Erreichen der prognostizierten Lebensdauer von 20 bis 30 Jahren Risse in der Blattschale auf. Die Folge sind aufwendige Reparaturen am installierten und schwer zugänglichen Rotorblatt und der kostenintensive Nutzungsausfall durch den Stillstand der WEA. Als mögliche Initiatoren für die Schäden in der Blattschale der Rotorblätter gelten fertigungsbedingte Imperfektionen. Für die Untersuchung des Einflusses dieser Imperfektionen auf das Ermüdungsverhalten der Rotorblätter wurde an der BAM (Bundesanstalt für Mate-rialforschung und -prüfung) ein Prüfstand für statische und zyklische Versuche von Schalensegmenten im intermediate scale entwickelt und betrieben. Die untersuchten Schalensegmente in Sandwichbauweise sind der Rotorblattschale von WEA im Hinblick auf die Strukturmechanik, die eingesetzten Halbzeuge, den Laminataufbau und dem eingesetzten Fertigungsverfahren ähnlich. Als Imperfektionen wurden verschiedenen Variationen von Lagenstößen in die Hautlagen und Schaumstöße mit Breitenvariation in den Stützkern reproduzierbar eingebracht. Die Überwachung des Schädigungszustandes während der Schwingversuche unter realistischen Lastszenarien erfolgt über eine kombinierte in situ Schädigungsüberwachung mittels passiver Thermografie und Felddehnungsmessung. Mit den durchgeführten Schwingversuchen und der begleitenden Überwachung des Schädigungszustandes ließen sich die Schadensinitiation und die signifikante Herabsetzung der Lebensdauer durch die eingebrachten Imperfektionen zweifelsfrei nachweisen und entsprechende Konstruktionshinweise für die betriebssichere Auslegung von Sandwichstrukturen ableiten. N2 - Wind turbines often exhibit cracks in the blade shells after only a few years in service, significantly before their expected 20 to 30 year design lifespan. This leads to complicated repairs on difficult to reach rotor blades, and can cause a cost-intensive standstill of the turbine. A possible source of these defects in the rotor blade shells are the imperfections which occur during production. In order to investigate the effect of these imperfections on the fatigue behavior of rotor blades, a test rig was developed at the BAM (Bundesanstalt für Materialforschung und -prüfung) upon which intermediate scale static and cyclic-fatigue testing could be performed. The complementary sandwich shell specimens developed and investigated with the test rig are representative of the outer shell of wind turbine rotor blades in terms of materials and manufacturing processes, as well as structural mechanics. The specimens were built with reproducible imperfections, including laminate overlaps in the face sheets and gaps of varying size in the foam core. The damage condition was monitored during cyclic-fatigue testing under realistic load cases using a combination of in-situ passive thermography and strain field measurement. The cyclic testing and parallel non-destructive structural health monitoring of the shell specimens showed the imperfections to significantly influence the damage initiation and decrease the component service life. The results can be used accordingly as recommendations for operationally more reliable design of sandwich structures. T3 - BAM Dissertationsreihe - 170 KW - Erneuerbare Energien KW - Windenergie KW - Verbundwerkstoffe KW - Betriebsfestigkeit KW - Komponentenprüfung KW - Renewable ernergy KW - Wind energy KW - Intermediate scale KW - Composites KW - Fatigue PY - 2022 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-546701 SN - 1613-4249 VL - 170 SP - 1 EP - 178 PB - Bundesanstalt für Materialforschung und -prüfung (BAM) CY - Berlin AN - OPUS4-54670 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Rizzardi, Q. A1 - McElfresh, C. A1 - Sparks, G. A1 - Stauffer, D. A1 - Marian, J. A1 - Maaß, Robert T1 - Mild-to-wild plastic transition is governed by athermal screw dislocation slip in bcc Nb N2 - Plastic deformation in crystals is mediated by the motion of line defects known as dislocations. For decades, dislocation activity has been treated as a homogeneous, smooth continuous process. However, it is now recognized that plasticity can be determined by longrange correlated and intermittent collective dislocation processes, known as avalanches. Here we demonstrate in body-centered cubic Nb how the long-range and scale-free dynamics at room temperature are progressively quenched out with decreasing temperature, eventually revealing intermittency with a characteristic length scale that approaches the Burgers Vector itself. Plasticity is shown to be bimodal across the studied temperature regime, with conventional thermally-activated smooth plastic flow (‘mild’) coexisting with sporadic Bursts (‘wild’) controlled by athermal screw dislocation activity, thereby violating the classical Notion of temperature-dependent screw dislocation motion at low temperatures. An abrupt increase of the athermal avalanche component is identified at the critical temperature of the material. Our results indicate that plasticity at any scale can be understood in terms of the coexistence of these mild and wild modes of deformation, which could help design better alloys by suppressing one of the two modes in desired temperature Windows. KW - Plastic deformation KW - Microplastic stress KW - Intermittent microplasticity PY - 2022 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-543927 DO - https://doi.org/10.1038/s41467-022-28477-4 VL - 13 IS - 1 SP - 1 EP - 9 PB - Nature AN - OPUS4-54392 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Ganesh, R. A1 - Gesell, Stephan A1 - Fedelich, Bernard A1 - Kuna, Meinhard A1 - Kiefer, B. T1 - Procrackplast: Eine Software zur Simulation des 3D-Risswachstums unter großen plastischen Deformationen T1 - Procrackplast: A software for simulating 3D crack growth under large plastic deformation N2 - The finite element software ProCrackPlast is developed for the automated simulation of fatigue crack growth in arbitrarily loaded three-dimensional components with large scale plastic deformations, in particular under cyclic thermomechanical (TMF) loading. ProCrackPlast is developed by extending the software Procrack, created at TU Freiberg for linear-elastic crack growth simulations. The pre-processing, FEM analysis, and the post-processing in ProCrackPlast are done by the commercial software ABAQUS. ProCrackPlast resorts to a crack growth procedure which adaptively updates the crack in finite increments based on the fracture-mechanical parameter, cyclic crack tip opening displacement ΔCTOD . Features of this software along with two application examples of fatigue crack growth in a typical cast steel, Ni-Resist, are presented in this paper to show its capability and performance. N2 - Es wird die Finite-Element-Software ProCrackPlast vorgestellt, die eine automatische Simulation der Ermüdungsrissausbreitung in beliebig belasteten dreidimensionalen Bauteilen mit größeren plastisch verformten Bereichen ermöglicht, insbesondere bei thermomechanischer Wechselbelastung (TMF). ProCrackPlast entstand durch Erweiterung des Programs ProCrack, das an der TU Freiberg für linear-elastische inkrementelle Rissfortschrittsanalysen entwickelt wurde. Das Pre-Processing, die FEM Analyse und das Post-Processing werden mit Hilfe der kommerziellen FE-Software ABAQUS durchgeführt. ProCrackPlast beruht auf einem Algorithmus, mit dem der Rissfortschritt adaptiv in endlichen Inkrementen unter Verwendung des bruchmechanischen Parameters der zyklischen Rissöffnungsverschiebung ΔCTOD gesteuert wird. Die Funktionseigenschaften dieser Software werden anhand von zwei Anwendungsbeispielen zum Ermüdungsrisswachstum für einen typischen Stahlguss, Ni-Resist, exemplarisch dargestellt, um die Möglichkeiten und Leistungsfähigkeit von ProCrackPlast zu demonstrieren. T2 - 54. Tagung des Arbeitskreises "Bruchmechanik und Bauteilsicherheit" CY - Online meeting DA - 22.02.2021 KW - Automated finite element analysis KW - Automatische Finite Element Simulation KW - Thermomechanical fatigue KW - Crack growth KW - Thermomechanische Ermüdung KW - Rissausbreitung PY - 2022 SP - 205 EP - 214 PB - Deutscher Verband für Materialforschung und -prüfung e.V. AN - OPUS4-54435 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Meyer, Lena A1 - Zocca, Andrea A1 - Wilbig, Janka A1 - Kolsch, Nico A1 - Günster, Jens T1 - Laser beam melting additive manufacturing at μ-gravity N2 - In-space manufacturing (ISM) provides the opportunity to manufacture and repair critical components on future human spaceflight missions. For explorations to Mars and beyond, ISM is a key strategy not only due to the long travel distances and high costs of supply from earth but also to be able to safely work in space for years. Human spaceflight is still dependent on shipments from earth that can fail for several reasons. ISM is a valuable alternative to ensure the timely and safe resupply of space missions. With additive manufacturing (AM) technologies, components are built directly from a 3D computer-aided-design (CAD) model which offers the advantages of freedom of design and the production of complex and ready-to-use parts. A virtual tool box with 3D models in space or the supply of information instead of components from earth to space can strongly benefit future missions. For industrial use, most research has focused on laser based additive manufacturing processes such as laser beam melting (LBM) where metallic powder particles are spread into a uniform powder bed and melted by a laser to the desired shape. In the absence of gravity, the handling of metal powders, which is essential for the process, is challenging. We present an evolution of an AM system, where a gas flow throughout the powder bed is applied to stabilize the powder bed. This is needed to compensate for the missing gravitational forces in microgravity experiments on parabolic flight campaigns. The system consists of a porous building platform acting as a filter for the fixation of metal particles in a gas flow. It is driven by reduced pressure established by a vacuum pump underneath the platform. The system creates a drag force that directs the particles towards the porous building platform, similar to the effect of the gravitational force. The AM system with its gas-flow-assisted powder deposition has been tested in several parabolic flight campaigns, and stainless-steel powder has successfully been processed during microgravity conditions. Different powder recoating mechanisms have been investigated to assess the homogeneous distribution of the powder as well as the attachment of the next layer to the powder bed. These mechanisms included different container designs with parallel double blades and with a V-shape at the bottom, and a roller recoating system. The samples presented are the first metal parts ever manufactured using LBM in μ-gravity. In addition to manufacturing in a μ-gravity environment, the experiments have shown the feasibility to manufacture components at different accelerations during the parabolic flight: hyper gravity (1.8 g), μ-gravity (< 0.01 g) and 1 g. Recent results will also be presented describing the application of this LBM setup in a parabolic flight campaign with mixed lunar, martian and µ-gravity acceleration, during which the processing of a lunar regolith simulant powder was tested. For ISM, the development and testing of the proposed AM system demonstrates that LBM can be considered a viable technology for the manufacturing of metal and ceramic parts in a μ-gravity or reduced-gravity environment. T2 - International Conference on Advanced Manufacturing CY - Online meeting DA - 07.03.2022 KW - μ-gravity KW - In-space manufacturing KW - Additive manufacturing KW - Laser beam melting KW - Microgravity KW - Stainless steel KW - Lunar regolith simulant PY - 2022 AN - OPUS4-54450 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Günster, Jens T1 - Research and carrier in governmental research institute in Japan and Germany N2 - Being invited to Japan in 1996 as a Humboldt/STA was on of the most exciting things in my life. Not that it is on an absolute scale the most exciting thing still, but at that time, just after finalizing my PhD and thinking what is coming next, it was. KW - Networking PY - 2022 DO - https://doi.org/10.11470/oubutsu.91.2_115 SN - 0369-8009 VL - 91 IS - 2 SP - 115 EP - 117 PB - Gakkai CY - Tōkyō AN - OPUS4-54462 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Agea, Boris A1 - Walzel, S. T1 - 3D Druck unterstütz die Dekarbonisierung N2 - Suspensionsbasiertes Binder Jetting reduziert die Brennzeiten von technischer Keramik im Vergleich zu anderen 3d-druckverfahren signifikant. dabei wird nicht nur Energie beim Betrieb der Brennöfen gespart, sondern auch die Emission von Kohlendioxid beim Brennvorgang selbst gesenkt. KW - Schlickerdeposition PY - 2021 VL - 6 SP - 26 EP - 28 PB - Keramische Zeitschrift AN - OPUS4-53812 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Blaeß, Carsten T1 - Viskose Rissschließung in Gläsern und Glasmatrixkompositen N2 - Um die Langzeitbeständigkeit von Hochtemperatur-Festoxidbrennstoffzellen (SOFC) sicherzustellen, ist das grundlegende Verständnis der viskosen Schließung oder Heilung von Rissen, als Folge wechselnder thermischer oder mechanischer Belastung, in Gläsern und teilkristallinen Materialien ein entscheidender Faktor. In Glas ist die Rissheilung hauptsächlich durch viskoses Fließen bestimmt. In teilkristallinen Schmelzen bewirkt der kristalline Volumenanteil die Erhöhung der effektiven Viskosität. Um die Auswirkungen des kristallinen Volumenanteils auf die Rissheilung zu ergründen, wurden Glasmatrixkomposite mit variierten inerten kristallinen Fülleranteilen, die während der Wärme-behandlung konstant blieben, hergestellt. Verwendet wurde ein kristallisationsträges Natrium-Calcium-Silicatglas und ZrO2 als inerter Füller. Komplexe, reproduzierbare Rissstrukturen wurden durch Vickers-Eindrücke erzeugt und die viskose Rissschließung während isothermer Wärmebehandlungs-schritte mittels Laser-Scanning-Mikroskopie verfolgt. Die Untersuchungen zeigen, dass, verglichen zum füllerfreien Glas, der kristalline Phasenanteil die effektive Viskosität erhöht und dadurch großräumiges Fließen verlangsamt. Dies verzögert das Aufweiten der Risse. Dieser Effekt erschwert die Rissverkürzung und führt oftmals zu großen gerundeten Kavitäten und dadurch zu einer verzögerten Rissschließung. Wird dieses Aufweiten verringert, ist zunächst ein lokales viskoses Fließen der Restglasphase weiterhin gegeben, sodass sich die Risse sogar schneller schließen. Für kristalline Anteile > 27 Vol% bildet sich dann ein stabiles Perkolationsgerüst aus, das die weitere Rissschließung auch lokal unterbindet. Nur innerhalb größerer glasiger Bereiche ist hierbei noch eine Rissschließung zu beobachten. Ein Optimum der Risslängenverkürzung konnte bei 17 Vol% beobachtet werden. T2 - 94. Glastechnische Tagung CY - Online meeting DA - 10.05.2021 KW - Glas KW - Hochtemperaturbrennstoffzelle KW - Glasmatrixkomposit KW - Rissheilung PY - 2021 AN - OPUS4-54245 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Feldmann, Titus A1 - Fedelich, Bernard A1 - Epishin, A. T1 - Simulation of Hot Isostatic Pressing in a Single-Crystal Ni Base Superalloy with the Theory of Continuously Distributed Dislocations Combined with Vacancy Diffusion N2 - Single-crystal components made of nickel base superalloys contain pores after casting and homogenization heat treatment. Hot isostatic pressing (HIP), which is carried above the γ' -solvus temperature of the alloy, is industrially applied to reduce porosity. A modeling of HIP based on continuously distributed dislocations is developed in a 2D setting. Glide and climb of straight-edge dislocations, as well as vacancy diffusion, are the deformation mechanisms taken into account. Thereby, dislocation glide is controlled by dragging a cloud of large atoms, and climb is controlled by vacancy diffusion. Relying on previous investigations of the creep behavior at HIP temperatures, it is assumed that new dislocations are nucleated at low-angle boundaries (LAB) and move through subgrains until they either reach the opposite LABs or react with other dislocations and annihilate. Vacancies are created at the pore surface and diffuse through the alloy until they are either consumed by climbing dislocations or disappear at the LABs. The field equations are solved by finite elements. It is shown that pore shrinking is mostly controlled by vacancy diffusion as the shear stresses at the LABs are too low to nucleate a sufficient amount of dislocations. KW - Nickel-base superalloys KW - HIP KW - Dislocation KW - Creep KW - Model PY - 2022 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-542309 DO - https://doi.org/10.1002/adem.202101341 VL - 2022 PB - Wiley AN - OPUS4-54230 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Viguier, B. A1 - Epishin, A. A1 - Fedelich, Bernard T1 - Creep of single-crystals of nickel-base gamma-alloy at high temperatures N2 - Porosity in single-crystal nickel-base superalloys is removed by hot isostatic pressing (HIP) at temperatures above gamma’-solvus where the material is very soft and ductile. For example, single-crystal nickel-base superalloy CMSX-4 is HIPed at temperature 1288 °C, which is slightly higher than the gamma’-solvus temperature of this alloy equal to about 1280 °C. It is assumed that pore shrinking during HIP is mostly due to dislocation creep. Such a modelling of HIP of CMSX-4 was started in our group on the base of results of creep tests of [001] single-crystals at 1288 °C [1]. However, it was found later [2] that the alloy CMSX-4 shows very strong creep anisotropy at 1288 °C. Therefore, for calibration of the creep law, creep tests of different orientations under different stress levels are required at the HIP temperature. This was the main task of present work. Single-crystals of CMSX-4 of axial orientations [001], [011], [123] and [111] were cast by VIAM Moscow and tested by BAM Berlin under creep conditions at 1288 °C and stress levels between 4 MPa and 16 MPa. At all stress levels, the creep rate increases by an order of magnitude when changing the orientation from [001] to [111] with [011] and [123] orientations in between. Such a character of creep anisotropy corresponds to the orientation dependence of the Schmid factor for octahedral glide. The crystal viscoplasticity model developed in [1] was improved to better represent the time induced softening observed during creep. The creep tests for different stresses and orientations as well as pore closure were simulated. The results of pore closure simulation are compared with measurements of porosity decrease during Hiping. T2 - 15th International Conference on Creep and Fracture of Engineering Materials and Structures CY - Online meeting DA - 14.06.2021 KW - Nickel-base superalloys KW - Creep KW - Single-Crystal PY - 2021 AN - OPUS4-53935 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Skrotzki, Birgit A1 - Olbricht, Jürgen A1 - Schilling, Markus A1 - Chen, Yue A1 - Füting, M. A1 - Todor, A. A1 - von Hartrott, P. A1 - Hanke, T. T1 - Wie digitalisieren wir die Werkstoffprüfung? Entwicklung standardisierter Versuchsbeschreibungen und Daten-Infrastrukturen in aktuellen Digitalisierungs-Initiativen N2 - Die Entwicklung digitaler Prozesse für die Materialwissenschaft und Werkstofftechnik muss naturgemäß auch die Charakterisierungsmethoden der Werkstoffprüfung abbilden, die oft durch eine hohe Komplexität gekennzeichnet sind. Als vorteilhaft erweist sich dabei der hohe Standardisierungsgrad, der sich z.B. in klaren Anforderungen an die eingesetzten Prüfmittel und festgelegten Vorgehensweisen ausdrückt. Diese können (und müssen) in entsprechenden digitalen Versuchsbeschreibungen abgebildet werden, wobei sich die klaren Datenstrukturen und Terminologien als vorteilhaft erweisen. T2 - Tagung Werkstoffprüfung 2021: Werkstoffe und Bauteile auf dem Prüfstand Prüftechnik – Kennwertermittlung – Schadensvermeidung CY - Online meeting DA - 02.12.2021 KW - Digitalisierung KW - Standardisierung KW - Normung KW - Ontologien KW - Wissensrepräsentation PY - 2021 AN - OPUS4-53943 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Kalinka, Gerhard T1 - Optische Beobachtungen der Faser-Matrix-Trennung im Pull-out-Versuch N2 - Der Vortrag behandelt Rissentstehung und Ausbreitung an Faser-Matrix-Interfaces, untersucht mit dem optischen Mikroskop. T2 - Composites United, CU-Arbeitsgruppe/n Faser-Matrix-Haftung & Matrices CY - Online meeting DA - 02.12.2021 KW - Faser KW - Matrix KW - Pull-out KW - Interface PY - 2021 AN - OPUS4-53968 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Ikeda, Yuki A1 - Yuan, R. A1 - Chakraborty, A. A1 - Ghassemi-Armaki, H. A1 - Zuo, J. M. A1 - Maaß, Robert T1 - Early stages of liquid-metal embrittlement in an advanced high-strength steel N2 - Grain-boundary degradation via liquid-metal embrittlement (LME) is a prominent and long-standing failure process in next generation advanced high-strength steels. Here we reveal, well ahead of the crack tip, the presences of nano-scale grains of intermetallic phases in Zn-infiltrated but uncracked grain boundaries with scanning- and 4D transmission electron microscopy. Instead of the often-reported Znrich Fe-Zn intermetallics, the nano-scale phase in the uncracked infiltrated grain boundaries is identified as the G-phase, and its presence reveals the local enhancement of strain heterogeneities in the grain boundary network. Based on these observations, we argue that intermetallic phase formation is not occurring after cracking and subsequent liquid Zn infiltration but is instead one of the primary nanoscopic drivers for grain-boundary weakening and crack initiation. These findings shift the focus of LME from micro- and meso-scale crack investigations to the very early stages immediately following Zn diffusion, after which secondary phase nucleation and growth emerge as the root-cause for failure. KW - Advanced high strength steels KW - Liquid metal embrittlement KW - Transmission electron microscopy KW - 4-Dimensional scanning transmission KW - electron microscopy PY - 2021 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-539716 DO - https://doi.org/10.1016/j.mtadv.2021.100196 SN - 2590-0498 VL - 13 IS - 196 SP - 1 EP - 8 PB - Elsevier Ltd. AN - OPUS4-53971 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Trappe, Volker T1 - Current and future technological advancement in polymer matrix composites enabled through fundamental discoveries N2 - This presentation is a summary of the work from the past 20 years’ development of PMC-testing at the BAM-FB 5.3 with respect to safety-relevant design of advanced light weight structures in aircraft, wind turbine and automotive applications. The talk begins with wood as an example from nature, and emphasizes that load case, fiber architectural design and the production process and quality have to go hand in hand to generate an advanced light weight structure. Since PMC-relevant basic findings of mankind span across hundreds of years, high-performance composite applications today are based more on long term experiences than on breakthrough inventions of modern days. In the second part of the talk, future plans and projects of FB-5.3 are presented, specifically addressing H2-safety, circular economy, recycling by design and digitalization of PMC-technologies. T2 - Abteilungsseminar CY - Online meeting DA - 07.09.2021 KW - Polymer Matrix Composites KW - Thermo mechanical fatigue PY - 2021 AN - OPUS4-54150 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Trappe, Volker T1 - Beschreibung des Ermüdungsverhaltens von Endlos-Faserverstärkten-Kunststoff-Verbunden mit Hilfe mikromechanischer Modelle N2 - Im Rahmen des Vortrags werden die neusten Ergebnisse aus dem Fachbereich 5.3 zur Beschreibung des Ermüdungsverhaltens von FKV mittels Mikromechanischer-Modelle präsentiert. Explizit wird der theoretische Ansatz am Beispiel von GFK unter thermomechanischer Beanspruchung hergeleitet und an Hand von Versuchsergebnissen verifiziert. T2 - Webkonferenz Composites United, Composite Fatigue CY - Online meeting DA - 30.09.2021 KW - Faser-Kunststoff-Verbunde KW - thermomechanische Beanspruchung KW - Materialmodell PY - 2021 AN - OPUS4-54151 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Derlet, P. A1 - Bocquet, H. A1 - Maaß, Robert T1 - Viscosity and transport in a model fragile metallic glass N2 - How thermally activated structural excitations quantitatively mediate transport and microplasticity in a model binary glass at the microsecond timescale is revealed using atomistic simulation. These local excitations, involving a stringlike sequence of atomic displacements, admit a far-field shear-stress signature and underlie the transport of free-volume and bond geometry. Such transport is found to correspond to the Evolution of a disclination network describing the spatial connectivity of topologically distinct bonding environments, demonstrating the important role of geometrical frustration in both glass structure and its underlying dynamics. KW - Metallic glass KW - Viscosity PY - 2021 DO - https://doi.org/10.1103/PhysRevMaterials.5.125601 SN - 2475-9953 VL - 5 SP - 1 EP - 7 PB - American Physical Society CY - College Park, MD AN - OPUS4-54152 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Chi, J. A1 - Agea Blanco, B. A1 - Bruno, Giovanni A1 - Günster, Jens A1 - Zocca, Andrea T1 - Self-Organization Postprocess for Additive Manufacturingin Producing Advanced Functional Structure and Material N2 - Additive manufacturing (AM) is developing rapidly due to itsflexibility in producing complex geometries and tailored material compositions. However, AM processes are characterized by intrinsic limitations concerning their resolution and surface finish, which are related to the layer-by-layer stacking process. Herein, a self-organization process is promoted as an approach to improve surface quality and achieve optimization of 3D minimal surface lightweight structures. The self-organization is activated after the powder bed 3D printing process via local melting, thereby allowing surface tension-driven viscous flow.The surface roughness Ra (arithmetic average of the roughness profile) could bedecreased by a factor of 1000 and transparent lenses and complex gyroid structures could be produced for demonstration. The concept of self-organization is further elaborated by incorporating external magnetic fields to intentionally manipulate magnetic particles, which are mixed with the polymer before printing and self-organization. This concept can be applied to develop programmable materials with specific microtextures responding to the external physical conditions. KW - Additive Manufacturing KW - Self-organization KW - Triply Periodical Minimal Surface PY - 2021 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-540588 DO - https://doi.org/10.1002/adem.202101262 VL - 24 IS - 6 SP - 1 EP - 8 PB - Wiley VCH AN - OPUS4-54058 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bresch, Harald A1 - Rühle, Bastian A1 - Hodoroaba, Vasile-Dan A1 - Resch-Genger, Ute A1 - Kuchenbecker, Petra A1 - Abram, Sarah-Luise A1 - Löhmann, Oliver A1 - Mrkwitschka, Paul T1 - Tour de table - BAM N2 - Kurzübersicht über die neuen Aktivitäten zu Nanomaterialien in 2021. T2 - Nano-Behördenklausur der Bundesoberbehörden 2021 CY - Online meeting DA - 17.11.2021 KW - Nano KW - Nanomaterial KW - Nanopartikel KW - Bundesoberbehörden PY - 2021 AN - OPUS4-53827 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Müller, Ralf A1 - Agea-Blanco, Boris A1 - Blaeß, Carsten A1 - Reinsch, Stefan A1 - Behrens, H T1 - Sintering and Foaming of Silicate Glass Powders N2 - The lecture focuses on the mechanisms of non-desired gas bubble formation and foaming during the sintering of glass powder compacts. It is shown that foaming is driven by carbon gases and that carbonates, encapsulated in micropores or mechaniacally dissolved beneath the glass surface, provide the major foaming source. T2 - Sandanski Workshop Sinter crystallization 27th-29th September 2021 PROJECT “THEORY AND APPLICATIONS OF SINTER-CYSTALLIZATION” DN 19/7 CY - Online meeting DA - 27.10. 2021 KW - Sintering KW - Non-desired foaming PY - 2021 AN - OPUS4-53772 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Zocca, Andrea A1 - Wilbig, Janka A1 - Waske, Anja A1 - Günster, Jens A1 - Widjaja, Martinus A1 - Neumann, C. A1 - Clozel, M. A1 - Meyer, A. A1 - Ding, J. A1 - Zhou, Z. A1 - Tian, X. T1 - Challenges in the Technology Development for Additive Manufacturing in Space N2 - Instead of foreseeing and preparing for all possible scenarios of machine failures, accidents, and other challenges arising in space missions, it appears logical to take advantage of the flexibility of additive manufacturing for “in-space manufacturing” (ISM). Manned missions into space rely on complicated equipment, and their safe operation is a great challenge. Bearing in mind the absolute distance for manned missions to the Moon and Mars, the supply of spare parts for the repair and replacement of lost equipment via shipment from Earth would require too much time. With the high flexibility in design and the ability to manufacture ready-to-use components directly from a computer-aided model, additive manufacturing technologies appear to be extremely attractive in this context. Moreover, appropriate technologies are required for the manufacture of building habitats for extended stays of astronauts on the Moon and Mars, as well as material/feedstock. The capacities for sending equipment and material into space are not only very limited and costly, but also raise concerns regarding environmental issues on Earth. Accordingly, not all materials can be sent from Earth, and strategies for the use of in-situ resources, i.e., in-situ resource utilization (ISRU), are being envisioned. For the manufacturing of both complex parts and equipment, as well as for large infrastructure, appropriate technologies for material processing in space need to be developed. KW - Additive manufacturing KW - Space KW - Process PY - 2022 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-549204 DO - https://doi.org/10.1016/j.cjmeam.2022.100018 SN - 2772-6657 VL - 1 IS - 1 SP - 1 EP - 13 PB - Elsevier Ltd. AN - OPUS4-54920 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Wang, Lei A1 - Hoyt, J. J. T1 - Layering misalignment and negative temperature dependence of interfacial free energy of B2-liquid interfaces in a glass forming system N2 - From molecular dynamics simulations and the capillary fluctuation method, the solid-liquid interfacial free energy has been computed for the B2-liquid interface in the Cu-Zr system. Consistent with previous results for the FCC-liquid interface in Cu-Zr and Al-Sm but atypical of most alloys, was found to increase as the temperature is lowered. In addition, the temperature dependence was obtained for model Lennard-Jones B2-liquid alloys. In all cases the unusual temperature dependence of is correlated with an atomic structure of the interfacial region characterized by a misalignment of the number density peaks between solvents and solutes. In cases where the number density peaks are aligned, the typical temperature dependence is observed. The results are discussed in terms of the Gibbs theory of the thermodynamics of interfaces. It is proposed that the unique interfacial structure and the atypical temperature dependence of are hallmarks of an easy glass forming alloy. KW - Atomistic simulations KW - Interfacial free energy KW - Layering misalignment KW - Glass forming PY - 2021 DO - https://doi.org/10.1016/j.actamat.2021.117259 SN - 1359-6454 VL - 219 SP - 117259 PB - Elsevier Ltd. AN - OPUS4-53650 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Abel, Andreas A1 - Zapala, P. A1 - Michels, H. A1 - Skrotzki, Birgit T1 - Microstructure-Property-Correlation of a Mo-Ti-B alloyed iron aluminide N2 - Iron aluminides depict a sustainable and light-weight material class which could be employed in many applications requiring high strength at intermediate to high temperatures. According to first results, the alloy Fe-26Al-4Mo-0.5Ti-1B surpasses conventional materials in wet corrosion resistance and creep resistance up to 650 °C. For these reasons, the AiF research project “WAFEAL – Materials applications for iron aluminides” was initiated to transfer these findings into a standardised materials dataset and to derive best practices for processing. In the first place, a set of different microstructures adjusted by varying casting methods, wall thicknesses and heat treatments was investigated and correlated with hardness on macro and micro scale. Correlations were drawn between solidification rates and resulting grain sizes and hardness. The effect of vacancy hardening was only verified for wall thickness as low as 2.5 mm. Moreover, a common decrease of macrohardness after a heat treatment at 1000 °C for 100 h was observed irrespective of casting process or wall thickness. This effect was linked with an unexpected decrease of the complex boride phase fraction which acts as a hardening phase. T2 - Intermetallics 2021 CY - Bad Staffelstein, Germany DA - 04.10.2021 KW - Fe-Al alloys KW - Intermetallics KW - Iron aluminides KW - Heat treatment KW - Wall thickness KW - Centrifugal casting KW - Die casting KW - Investment casting KW - Microstructure KW - Hardness KW - Complex borides PY - 2021 AN - OPUS4-53617 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Thuy, Maximilian A1 - Niebergall, Ute A1 - Böhning, Martin T1 - Umgebungsbedingter Spannungsriss: Gefahr für Kunststoffbauteile unter Medieneinfluss N2 - Polyethylen hoher Dichte (PE-HD) ist ein weit verbreitetes Material für Transportbehälter, die oft für eine längere Nutzungsdauer vorgesehen sind. Insbesondere in diesem Fall können mikroskopische Schäden im Material auch weit unterhalb der Streckgrenze auftreten, die durch eine Spannungskonzentration verursacht werden, deren Ursprung in intrinsischen Materialfehlern oder äußeren Kratzern liegt. Mit fortschreitender Schädigung bilden sich Rissstrukturen, die von verstreckten Fibrillen aufgespannt werden, bis es zum Versagen dieser Fibrillen kommt und sich der Riss ausbreitet. Dieser Schadensmechanismus des langsamen Risswachstums kann durch eine Vielzahl von Umgebungsmedien beschleunigt werden und wird dann als "environmental stress cracking" (ESC) bezeichnet. Eine international normierte Methode zur Validierung der Spannungsrissbeständigkeit von PE-HD Materialien ist der „Full Notch Creep Test“ (FNCT). Anhand von Bruchflächenauswertungen mittels Rasterelektronenmikroskopie und Laser-Scanning-Mikroskopie, werden die typischen Schädigungsstrukturen des ESC sichtbar. Die fibrillierten Strukturen des ESC auf der Bruchfläche von PE-HD ergeben sich besonders bei oberflächenaktiven wässrigen Umgebungsmedien. In Lösungsmittel-Umgebungsmedien, im Zusammenspiel mit PE-HD, kommt es aufgrund der plastifizierenden Wirkung zur Herabsetzung der Streckspannung und Bruchflächen aus dem FNCT veranschaulichen keine signifikanten Anzeichen des Schädigungsmechanismus ESC. T2 - 47. VDI-Jahrestagung Schadensanalyse 2021- Mediale und klimatische Beanspruchung von polymeren Produkten CY - Würzburg, Germany DA - 06.10.2021 KW - Umgebungsbedingter Spannungsriss KW - Polyethylen hoher Dichte KW - Full Notch Creep Test KW - Lösungsmittel KW - Oberflächenaktive wässrige Medien KW - Bruchflächenauswertung PY - 2021 AN - OPUS4-53665 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Gebhardt, M. A1 - Malolakis, I. A1 - Kalinka, Gerhard A1 - Deubener, J. A1 - Chakraborty, S. A1 - Meiners, D. T1 - Re-use potential of carbon fibre fabric recovered from infusible thermoplastic CFRPs in 2nd generation thermosetting-matrix composites N2 - The research presented here attempts to assess the potential for re-using carbon fibre (CF) fabrics recovered from recycling infusible acrylic thermoplastic carbon fibre reinforced polymer composites (CFRPs) in a universal manner, i.e. by combining with a wide variety of matrices to manufacture 2nd generation composite laminates by resin infusion. The 2nd generation composites have been compared in terms of bulk and interfacial properties against counteparts processed with virgin carbon fibre fabric infused with the same matrices. Generally, an increase in damping (tanδ) was observed in all 2nd generation composites, which can be attributed to a residual thin thermoplastic layer present on the recovered fibres. The interfacial adhesion of the 2nd generation Composites was investigated by shear tests and scanning electron micsoscopy, and also appears to be less influenced by the type of matrix. KW - Composite recycling KW - Thermoplastic matrix KW - Thermosetting resin KW - Fibre/matrix bonding PY - 2021 DO - https://doi.org/10.1016/j.coco.2021.100974 VL - 28 SP - 100974 PB - Elsevier Ltd. CY - Niederlande AN - OPUS4-53639 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Tielemann, Christopher A1 - Busch, R. A1 - Reinsch, Stefan A1 - Patzig, C. A1 - Höche, T. A1 - Avramov, I. A1 - Müller, Ralf T1 - Oriented surface nucleation in diopside glass N2 - Es wird die Texturbildung in kristallisierendem Diopsidglas im Zusammenhang mit der Oberflächenbeschaffenheit der unbehandelten Probe untersucht. Zudem wird der diskutiert, dass es sich bei der Texturbildung in Gläsern höchstwahrscheinlich um ein Nukleationsphänomen handelt welches auf die richtungsabhängige Grenzflächenenergie der kristallisierenden Phase zurückzuführen ist. N2 - Oriented surface crystallization on polished diopside glass surfaces has been studied with scanning electron microscopy, electron backscatter diffraction, transmission electron microscopy and laser scanning microscopy. An orientation preference of [001] parallel to the glass surface was detected for separately growing diopside crystals even as small as 700 nm in size. This finding shows that crystal orientation occurs in the outermost surface layer without crystal-crystal interaction and indicates that the crystal orientation is a result of oriented nucleation. Depending on surface preparation, monomodal crystal orientation distributions with [100] perpendicular to the surface or bimodal distributions with [100] and [010] perpendicular to the glass Surface were detected. It was also shown that the degree of crystal orientation increases with decreasing Surface roughness. The observed orientation of diopside crystals could be explained in terms of the interfacial energies of different crystal faces. KW - Surface energy KW - Glass ceramic KW - Glass KW - EBSD KW - Diopsid PY - 2021 UR - https://www.sciencedirect.com/science/article/pii/S002230932100020X DO - https://doi.org/10.1016/j.jnoncrysol.2021.120661 SN - 0022-3093 VL - 562 PB - Elsevier B.V. AN - OPUS4-53073 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CHAP A1 - Stephan-Scherb, Christiane ED - Schorr, S. ED - Weidenthaler, C. T1 - Crystallographic challenges in corrosion research N2 - High-temperature corrosion is a widespread problem in various industries. As soon as a hot and reactive gas (CO2, O2, H2O, SO2, NOx, etc.) is in contact with a solid, physico-chemical processes at the surface and interfaces lead to material degradation. The processes are dynamic and controlled by thermodynamic and kinetic boundary conditions. Whether a reaction product is protective or not depends on various factors, such as chemical composition of the solid and the reactive media, surface treatment as well as diffusion and transport paths of cations and anions. Resulting chemical and structural inhomogeneities with the corrosion layers are characterized by off stoichiometry within cationic and anionic sub lattices. The competitive processes can be studied by various techniques of applied crystallography. This chapter gives an overview on the challenges of chemical-structural Analysis of reaction products by crystallographic methods such as X-ray diffraction and X-ray near-edge structure spectroscopy and scanning electron microscopy electron backscatter diffraction (SEM-EBSD) for corrosion science. KW - High-temperature corrosion KW - Oxidation KW - Diffraction KW - Spectroscopy KW - Oxides PY - 2021 DO - https://doi.org/10.1515/9783110674910-009 SP - 291 PB - De Gruyter ET - 1 AN - OPUS4-52903 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Trappe, Volker A1 - Kraus, David T1 - Thermo-mechanical fatigue of glass fiber reinforced polymer N2 - Glass fiber reinforced polymer (GFRP) materials in practical applications have to endure cyclic mechanical loading in a wide temperature range (e.g. aircraft applications, automotive, wind turbine blades). In this study the static strength and fatigue behavior of GFRP was investigated in a temperature range from 213 K to 343 K. Therefor the coefficients of thermal expansion of the composite as well as the matrix are measured in this temperature interval. The inverse laminate theory was extended and used to calculate the inter fiber-failure effort for a virtual UD-layer according to the layer wise strength approach. The experimentally determined results are compared with the micro-mechanical model according to Krimmer, which has been enhanced to include the effect of temperature and fiber-perpendicular failure modes. A correlation between matrix effort, the dilatational strain energy of the matrix and the damage state of the specimen is demonstrated. It is shown that a fatigue life assessment can be performed with the aid of a temperature-independent master fatigue curve, as it was similar done for the fatigue behavior of CFRP and GFRP to very high load cycles at room temperature. T2 - ICFC8 - The 8th International Conference on the Fatigue of Composites CY - Online meeting DA - 23.06.2021 KW - Glass fibre reinforced plastics KW - Fatigue KW - Thermo-mechanical-loading PY - 2021 AN - OPUS4-52910 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Skrotzki, Birgit A1 - Schriever, Sina T1 - BAM reference data - Results of ASTM E139-11 creep tests on a reference material of Nimonic 75 nickel-base alloy N2 - Results of creep tests on a certified reference material at T = 600°C and a tensile creep load of 160 MPa are provided. The evaluated results include the times to reach 2% and 4% creep strain, respectively, and the creep rate after 400 h. The data were audited and are BAM reference data. KW - Reference data KW - Creep KW - Nickel-base alloy KW - Nimonic 75 KW - Reference material BCR-425 PY - 2021 DO - https://doi.org/10.5281/zenodo.5106606 PB - Zenodo CY - Geneva AN - OPUS4-52970 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Heuser, Lina A1 - Nofz, Marianne A1 - Müller, Ralf A1 - Deubener, J. T1 - Sintering of silver‑alkali zinc borate glass‑composites N2 - Since decades electric contacts based on silver metallization pastes are key components of photovoltaics and advanced microelectronics. For the metallization of commercial Si solar cells, high conductive silver glass pastes are cost effectively applicated by screen printing. Nevertheless, silver pastes are still one of the most crucial and expensive none Si materials in solar cells. Ever shorter time to market as well as increasing demands on reduced Ag consumption and line width require the targeted development of silver-glass-pastes with increased sinter ability and electrical conductivity. As a main difficulty, however, the liquid phase sintering of silver glass pastes is poorly understood so far. In the present study, the influence of different network modifier in alkali-zinc-borate paste glasses on liquid phase sintering of silver-glass-pastes was investigated. Low melting X2O-ZnO-B2O3 glasses with X = Na, Li and Rb (abbr. LZB, NZB, and RZB) were utilized to prepare silver-glass-composites containing 30 %Vol glass. Shrinkage behavior of the silver-glass-composites compared with that of pure silver and pure glass powder compacts was studied with heating microscopy. The powder compacts were uniaxially pressed and heated at 5 K/min to the glass softening temperature. Glass transformation temperature and viscosity of the glasses were respectively measured with dilatometry and rotational viscometry. The thermal behavior of the pure glasses was analyzed with thermal analysis. Additionally, the contact angle of glass on pure silver foil was determined by means of heating microscopy between room temperature and 830 °C. Thermal analysis of the alkali-zinc-borate-glasses under study has shown transformation temperatures between 450 °C (RZB), 460 °C (LZB) and 465 °C (NZB). For all glasses crystallization was found to start approximately at about 550 °C. However, different peak areas hint on a different degree of crystallization. Conformingly, the sintering behavior, measured in terms of area shrinkage, significantly differed for the silver-pastes under study. For silver-pastes with NZB or LZB-glass, sintering starts at 464 °C for NZB Ag pastes and at 451 °C for LZB Ag pastes and ends at 597 °C for NZB Ag paste and at 594 °C for LZB Ag paste. The sintering of the RZB Ag paste proceeds between 426 °C and 703 °C. The final densification was retarded possibly due to crystallization or swelling. The low sinter onset at 426 °C seems to correlate with the good wetting behavior of the RZB glass. Thus, the lowest apparent contact angle between the just densified powder compact sintered at a silver substrate was found for this glass. Moreover, microstructure analyses of the various composites indicate differences in silver dissolution and reprecipitation. T2 - Technology Crossover Extravaganza, HiTEC/CICMT/APEPS CY - Online meeting DA - 26.04.2021 KW - Silver-glass-metallization-paste KW - Sintering KW - Crystallization KW - Alkali ions KW - Sintering atmosphere PY - 2021 AN - OPUS4-52872 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Busch, R. A1 - Tielemann, Christopher A1 - Reinsch, Stefan A1 - Müller, Ralf A1 - Patzig, C. A1 - Krause, M. A1 - Höche, T. T1 - Sample preparation for analytical scanning electron microscopy using initial notch sectioning N2 - A novel method for broad ion beam based sample sectioning using the concept of initial notches is presented. An adapted sample geometry is utilized in order to create terraces with a well-define d step in erosion depth from the surface. The method consists of milling a notch into the surface, followed by glancing-angle ion beam erosion, which leads to preferential erosion at the notch due to increased local surface elevation. The process of terrace formation can be utilized in sample preparation for analytical scanning electron microscopy in order to get efficient access to the depth-dependent microstructure of a material. It is demonstrated that the method can be applied to both conducting and non-conducting specimens. Furthermore, experimental parameters influencing the preparation success are determined. Finally, as a proof-of-concept, an electron backscatter diffraction study on a surface crystallized diopside glass ceramic is performed, where the method is used to analyze orientation dependent crystal growth phenomena occurring during growth of surface crystals into the bulk. KW - 3D etching KW - Ion beam erosion Sectioning KW - EBSD KW - Sample preparation KW - Analytical scanning electron microscopy KW - SEM KW - Glass Ceramic KW - Glass KW - Diopsid PY - 2021 DO - https://doi.org/10.1016/j.micron.2021.103090 SN - 0968-4328 VL - 150 PB - Elsevier B.V. AN - OPUS4-53075 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Ikeda, Yuki A1 - Nishijima, M. A1 - Kiguchi, T. A1 - Konno, T. T1 - Crystal structure characterization of martensite of Cu–Zn–Al ternary alloy by spherical aberration corrected scanning transmission electron microscopy N2 - The crystal structure of martensite in Cu-27at.%Zn-9.0 at.%Al alloy has been studied by using sphericalaberration-corrected high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) and geometrical phase analysis (GPA) to examine possible changes in atomic rearrangements during martensitic transformation of this ternary system. Observation along [100]M zone axis is suitable for examining a chemical order of the martensite, and showed that, despite the non-stoichiometry of the alloy, atomic columns containing Al atoms are imaged and distinguished from the others. On the other hand, observation along [010]M zone axis directly revealed that the parent and martensitic phases possess L21 and 18R (21) structures, respectively. These observations suggested that the martensite retained the local chemical order of the parent phase without shuffling before and after the transformation. GPA revealed that the interface between the two phases was coherent with tilting of the basal plane approximately 6◦ across the boundary, which makes otherwise large inclination small during the martensitic transformation. KW - Shape-memory alloys KW - Martensitic transformation KW - Martensitic structure KW - Electron microscopy, transmission PY - 2021 DO - https://doi.org/10.1016/j.intermet.2021.107286 SN - 0966-9795 VL - 137 PB - Elsevier Ltd. AN - OPUS4-53076 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Qu, R. A1 - Maaß, Robert A1 - Liu, Z. A1 - Tönnies, D. A1 - Tian, L. A1 - Ritchie, R. A1 - Zhang, Z. A1 - Volkert, A. T1 - Flaw-insentive fracture of a micrometer-sized brittle metallic glass N2 - Brittle materials, such as oxide glasses, are usually very sensitive to flaws, giving rise to a macroscopic fracture strength that is much lower than that predicted by theory. The same applies to metallic glasses (MGs), with the important difference that these glasses can exhibit certain plastic strain prior to catas- trophic failure. Here we consider the strongest metallic alloy known, a ternary Co 55 Ta 10 B 35 MG. We show that this macroscopically brittle glass is flaw-insensitive at the micrometer scale. This discovery emerges when testing pre-cracked specimens with self-similar geometries, where the fracture stress does not de- crease with increasing pre-crack size. The fracture toughness of this ultra-strong glassy alloy is further shown to increase with increasing sample size. Both these findings deviate from our classical under- standing of fracture mechanics, and are attributed to a transition from toughness-controlled to strength- controlled fracture below a critical sample size. KW - Metallic glass KW - Fracture toughness KW - Size effect KW - Small-scale PY - 2021 DO - https://doi.org/10.1016/j.actamat.2021.117219 VL - 218 PB - Elsevier Ltd. AN - OPUS4-53097 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Müller, Ralf A1 - Behrens, Harald A1 - Ageo-Blanco, Boris A1 - Reinsch, Stefan A1 - Wirth, Thomas T1 - Foaming Species and Trapping Mechanisms in Barium Silicate Glass Sealants N2 - Barium silicate glass powders 4 h milled in CO2 and Ar and sintered in air are studied with microscopy, total carbon analysis, differential thermal Analysis (DTA), vacuum hot extraction mass spectroscopy (VHE-MS), Fourier-transformed infrared (FTIR) spectroscopy, X-ray photoelectron spectroscopy (XPS), and time-of-flight secondary-ion mass spectrometry (TOF-SIMS). Intensive foaming of powder compacts is evident, and VHE studies prove that foaming is predominantly caused by carbonaceous species for both milling gases. DTA Shows that the decomposition of BaCO3 particles mix-milled with glass powders occurs at similar temperatures as foaming of compacts. However, no carbonate at the glass surface could be detected by FTIR spectroscopy, XPS, and TOF-SIMS after heating to the temperature of sintering. Instead, CO2 molecules unable to rotate identified by FTIR spectroscopy after milling, probably trapped by mechanical dissolution into the glass bulk. Such a mechanism or microencapsulation in cracks and particle aggregates can explain the contribution of Ar to foaming after intense milling in Ar atmosphere. The amount of CO2 molecules and Ar, however, cannot fully explain the extent of foaming. Carbonates mechanically dissolved beneath the surface or encapsulated in cracks and micropores of particle aggregates are therefore probably the major foaming source. KW - Milling KW - Foaming KW - Glass powder KW - Sintering PY - 2021 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-531227 DO - https://doi.org/10.1002/adem.202100445 SN - 1438-1656 VL - 24 IS - 6 SP - 2100445-1 EP - 2100445-13 AN - OPUS4-53122 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Epishin, A. I. A1 - Fedelich, Bernard A1 - Viguier, B. A1 - Schriever, Sina A1 - Svetlov, I. L. A1 - Petrushin, N. V. A1 - Saillard, R. A1 - Proietti, A. A1 - Poquillon, D. A1 - Chyrkin, A. T1 - Creep of single-crystals of nickel-base γ-alloy at temperatures between 1150 °C and 1288 °C N2 - A γ-analogue of the superalloy CMSX-4 that does not contain the strengthening γ′ -phase and only consists of the γ-solid solution of nickel has been designed, solidified as single-crystals of different orientations, and tested under creep conditions in the temperature range between 1150 and 1288 °C. The tests have revealed a very high creep anisotropy of this alloy, as was previously found for CMSX-4 at supersolvus temperature of 1288 °C. This creep anisotropy could be explained by the dominance of 〈011〉{111} octahedral slip. Furthermore, the analysis of the creep data has yielded a high value of the creep activation energy, Qc≈442 kJ/mol, which correlates with the high activation energy of Re diffusion in Ni. This supports the hypothesis that dislocation motion in the γ-matrix of Re-containing superalloys is controlled by the diffusion of the Re atoms segregating at the dislocation core. The Norton stress exponent n is close to 5, which is a typical value for pure metals and their alloys. The absence of γ′ -reprecipitation after high-temperature creep tests facilitates microstructural investigations. It has been shown by EBSD that creep deformation results in an increasing misorientation of the existing low angle boundaries. In addition, according to TEM, new low angle boundaries appear due to reactions of the a/2 〈011〉 mobile dislocations and knitting of new networks. KW - Nickel alloys KW - Single-crystals KW - Creep KW - Electron microscopy KW - Deformation mechanisms PY - 2021 DO - https://doi.org/10.1016/j.msea.2021.141880 SN - 0921-5093 VL - 825 SP - 1 EP - 13 PB - Elsevier CY - Amsterdam AN - OPUS4-53132 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Diener, S. A1 - Zocca, Andrea A1 - Günster, Jens T1 - Literature review: Methods for achieving high powder bed densities in ceramic powder bed based additive manufacturing N2 - In additive manufacturing the powder bed based processes binder jetting and powder bed fusion are increasingly used also for the production of ceramics. Final part properties depend to a high percentage on the powder bed density. Therefore, the aim is to use the best combination of powder deposition method and powder which leads to a high packing of the particles. The influence of flowability, powder properties and deposition process on the powder bed density is discussed and the different deposition processes including slurry-based ones are reviewed. It turns out that powder bed density reached by slurry-based layer deposition exceeds conventional powder deposition, however, layer drying and depowdering are extra steps or more time-consuming for the slurry route. Depending on the material properties needed the most suitable process for the part has to be selected. KW - Additive Manufacturing KW - Powder-based processes KW - Powder bed density PY - 2021 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-534992 DO - https://doi.org/10.1016/j.oceram.2021.100191 VL - 8 SP - 100191 PB - Elsevier Ltd. AN - OPUS4-53499 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Schilling, Markus A1 - Skrotzki, Birgit A1 - Olbricht, Jürgen T1 - Ansätze zur digitalen Wissensrepräsentation aus der Plattform MaterialDigital (PMD) N2 - Die Digitalisierung von Materialien und Prozessen stellt eine große Herausforderung dar, die nur durch eine Bündelung der Bemühungen aller Beteiligten in diesem Bereich erreicht werden kann. Bei einer derartigen digitalen Beschreibung spielen Datenanalysemethoden, eine Qualitätssicherung von Prozessen inklusive Input- und Output-Daten sowie die Interoperabilität zwischen Anwendungen nach den FAIR-Prinzipien eine wichtige Rolle. Dies umfasst das Speichern, Verarbeiten und Abfragen von Daten in einer vorzugsweise standardisierten Form (Beteiligung von Normungsgremien). Zur Bewältigung dieser Herausforderung ist eine mit allen Stakeholdern konsistente Kontextualisierung der Materialdaten anzustreben, d.h. alle erforderlichen Informationen über den Zustand des Materials einschließlich produktions- und anwendungsbezogener Änderungen müssen über eine einheitliche, maschinenlesbare Beschreibung verfügbar gemacht werden. Dazu werden Wissensrepräsentationen und Konzeptualisierungen ermöglichende Ontologien verwendet. Eine zentrale Betrachtungsweise in diesem Zusammenhang ist die Realisierung von (automatisierten) Datenpipelines, die eine Beschreibung und Verfolgung von Daten ausgehend von ihrer Erzeugung, bspw. in einem Messgerät, bis zu ihrer globalen Verwendung in möglicherweise verschiedenen Kontexten beinhalten. Erste Bemühungen und Ansätze zu diesen Problemstellungen führten im Projekt Innovations-Plattform Material Digital (PMD, materialdigital.de) zur Erstellung von Anwendungsontologien, die Prozesse und Testmethoden explizit beschreiben. Dabei wurde u.a. der Zugversuch an Metallen bei Raumtemperatur nach ISO 6892-1 ontologisch beschrieben. Diese als Beispiel dienende Ontologieentwicklung wird in dieser Präsentation vorgestellt. Weiterhin wurde, ausgehend von der domänenspezifischen Entwicklung von Anwendungsontologien, eine Kernontologie erstellt, die eine übergeordnete Verbindung von ontologischen Konzepten aufgrund der Verwendung gleichen Vokabulars und semantischer Verknüpfungen erlaubt. Diese sowie die das PMD-Projekt selbst werden ebenfalls in dieser Präsentation vorgestellt. T2 - DVM Workshop: Grundlagen und Beispiele zur Digitalisierung für die Materialforschung und -prüfung CY - Online meeting DA - 19.10.2021 KW - Plattform Material Digital (PMD) KW - Ontologie KW - Zugversuch KW - Wissensrepräsentation KW - Semantic Web PY - 2021 AN - OPUS4-53565 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Schilling, Markus A1 - Niebergall, Ute A1 - Marschall, Niklas A1 - Alig, I. A1 - Böhning, Martin T1 - A phenomenological criterion for an optical assessment of PE-HD fracture surfaces obtained from FNCT N2 - The full-notch creep test (FNCT) is a common test method to evaluate the environmental stress cracking (ESC) behavior of high-density polyethylene (PE-HD), e.g. for container materials. The test procedure as specified in ISO 16770 provides a comparative measure of the resistance against ESC using the time to failure of PE-HD specimens under constant mechanical load in a well-defined liquid test environment. Since the craze-crack damage mechanism underlying the ESC phenomenon is associated with brittle failure, the occurrence of a predominantly brittle fracture surface is a prerequisite to consider an FNCT measurement as representative for ESC, i.e. a time to failure dominated by craze-crack propagation. The craze-crack propagation continuously reduces the effective residual cross-sectional area of the specimen during the test, which results in a corresponding increase of the effective mechanical stress. Thus, a transition to ductile shear deformation is inevitable at later stages of the test, leading usually to a pronounced central ligament. Therefore, an optical evaluation of FNCT fracture surfaces concerning their brittleness is essential. An enhanced imaging analysis of FNCT fracture surfaces enables a detailed assessment of craze-crack Propagation during ESC. In this study, laser scanning microscopy (LSM) was employed to evaluate whether FNCT fracture surfaces are representative with respect to craze-crack propagation and ESC. Based on LSM height data, a phenomenological criterion is proposed to assess the validity of distinct FNCT measurements. This criterion is supposed to facilitate a quick evaluation of FNCT results in practical routine testing. Its applicability is verified on a sample basis for seven different commercial PE-HD container materials. KW - Environmental stress cracking (ESC) KW - Full notch creep test (FNCT) KW - Laser scanning microscopy (LSM) KW - Fracture surfaces KW - Optical criterion of brittleness PY - 2021 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-521012 DO - https://doi.org/10.1016/j.polymertesting.2020.107002 VL - 94 SP - 107002 PB - Elsevier Ltd. CY - Amsterdam AN - OPUS4-52101 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Kindrachuk, Vitaliy A1 - Klunker, Andre T1 - Phase field modeling of Hertzian cone cracks under spherica indentation N2 - A phase field model of brittle fracture has been developed to simulate the Hertzian crack induced by penetration of a rigid sphere to an isotropic linear-elastic half-space. The fracture formation is regarded as a diffusive field variable, which is zero for the intact material and unity if there is a crack. Crack growth is assumed to be driven by a strain invariant. The numerical implementation is performed with the finite element method and an implicit time integration scheme. The mechanical equilibrium and the phase field equations are solved in a staggered manner, sequentially updating the displacement field and the phase field variable. Numerical examples demonstrate the capability of the model to reproduce the nucleation and growth of the Hertzian cone crack. KW - Hertzian cracks KW - Phase field model KW - Contact mechanics PY - 2021 DO - https://doi.org/10.1007/s11223-021-00251-9 VL - 52 IS - 6 SP - 967 EP - 974 AN - OPUS4-52276 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Plarre, Rüdiger A1 - Zocca, Andrea A1 - Spitzer, Andrea A1 - Benemann, Sigrid A1 - Gorbushina, Anna A1 - Li, Y. A1 - Waske, Anja A1 - Funk, Alexander A1 - Wilgig, Janka A1 - Günster, Jens T1 - Searching for biological feedstock material: 3D printing of wood particles from house borer and drywood termite frass N2 - Frass (fine powdery refuse or fragile perforated wood produced by the activity of boring insects) of larvae of the European house borer (EHB) and of drywood termites was tested as a natural and novel feedstock for 3D-printing of wood-based materials. Small particles produced by the drywood termite Incisitermes marginipennis and the EHB Hylotrupes bajulus during feeding in construction timber, were used. Frass is a powdery material of particularly consistent quality that is essentially biologically processed wood mixed with debris of wood and faeces. The filigree-like particles flow easily permitting the build-up of woodbased structures in a layer wise fashion using the Binder Jetting printing process. The Quality of powders produced by different insect species was compared along with the processing steps and properties of the printed parts. Drywood termite frass with a Hausner Ratio HR = 1.1 with ρBulk = 0.67 g/cm3 and ρTap = 0.74 g/cm3 was perfectly suited to deposition of uniformly packed layers in 3D printing. We suggest that a variety of naturally available feedstocks could be used in environmentally responsible approaches to scientific material sciences/additive manufacturing. KW - 3D printing KW - X-ray tomographic KW - SEM micrography KW - Drywood termite PY - 2021 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-521517 DO - https://doi.org/10.1371/journal.pone.0246511 VL - 16 IS - 2 SP - e0246511 AN - OPUS4-52151 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - THES A1 - Kraus, David T1 - Ermüdungsverhalten von Glasfaser-Kunststoff-Verbunden unter thermomechanischer Beanspruchung N2 - Die Werkstoffgruppe der Faser-Kunststoff-Verbunde (FKV) hat sich aufgrund ihrer hervorragenden Leichtbaueigenschaften unter anderem im Sportgerätebau, in der Luft- und Raumfahrt und in der Windenergieindustrie etabliert. Die so hergestellten Strukturen sind in der Regel nicht nur mechanischen Belastungen, sondern auch thermischen Lasten in einem breiten Temperaturspektrum ausgesetzt. Dennoch ist die Auswirkung des Temperatureinflusses bei einer Kombination von thermischer und mechanischer Last auf die Lebensdauer von Strukturen aus FKV bisher nur wenig untersucht. Im Rahmen dieser Arbeit wird der Einfluss von Temperaturen zwischen 213 K und 343 K auf einen Glasfaser-Epoxidharz-Verbund experimentell untersucht. Das Material wird in diesem Temperaturbereich eingehend charakterisiert: Es werden sowohl die thermomechanischen Eigenschaften von Faser- und Matrixwerkstoff als auch die des Verbundes ermittelt. In einem weiteren Schritt wird dann der Einfluss der Temperatur auf die Schädigungsentwicklung im quasi-statischen Lastfall sowie unter schwingender Ermüdungsbeanspruchung bei verschiedenen FKV-Mehrschichtverbunden analysiert. Basierend auf den experimentellen Daten wird ein Zusammenhang zwischen der Schädigung und der Anstrengung der Matrix innerhalb der Einzelschicht demonstriert. Die Matrixanstrengung wird mithilfe eines mikromechanischen Modells unter Berücksichtigung der thermomechanischen Eigenspannungen analytisch berechnet. Bei Querzugbeanspruchung kann gezeigt werden, dass eine Vorhersage der Schädigung in Abhängigkeit der Volumenänderungsenergie innerhalb der Matrix getroffen werden kann. Mithilfe des Konzepts der Matrixanstrengung ist eine Vorhersage der Lebensdauer des Werkstoffs unter schwingender Ermüdungsbeanspruchung in Abhängigkeit der Einsatztemperatur möglich. N2 - Due to their superior lightweight properties, fiber reinforced polymer (FRP) materials are well established in various fields, such as sports equipment, aerospace or wind energy structures. These structures are not only subjected to mechanical loads, but also to a broad spectrum of thermal environments. However, the impact of temperature on the fatigue life of thermomechanically loaded FRP structures is barely investigated to-date. In the scope of this work, the influence of temperatures in a range of 213 K to 343 K on a glass fiber reinforced epoxy polymer is experimentally examined. An extensive thermo-mechanical characterization of the static properties of the material is performed. The neat resin and Fiber material are investigated, as well as the composite. In addition, the impact of thermal loads on the damage evolution under quasi-static as well as cyclic fatigue loading is investigated for different multi-angle laminates. Based on the experimental data, a correlation is shown between damage and matrix effort of the unidirectional layer. The matrix effort is calculated according to a micromechanical model considering thermal residual stresses. Particularly under transverse loading, the damage Evolution can be predicted as a function of the dilatational strain energy of the matrix. Using the concept of the matrix effort presented in this work, a prediction of the fatigue life of the investigated material at different ambient temperature conditions can be performed. T3 - BAM Dissertationsreihe - 169 KW - Ermüdung KW - Faser-Kunststoff-Verbund KW - GFK KW - Schädigung KW - Thermomechanik KW - Fatigue KW - Composite KW - Glas fibre reinforced polymer KW - Damage KW - Thermomechanics PY - 2021 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-530253 SN - 1613-4249 VL - 169 SP - 1 EP - 164 PB - Bundesanstalt für Materialforschung und -prüfung (BAM) CY - Berlin AN - OPUS4-53025 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Hmood, F. J. A1 - Wilbig, Janka A1 - Nicolaides, Dagmar A1 - Zocca, Andrea A1 - Günster, Jens T1 - An approach to monitor the real-time deformation during heat treatment of 3D-printed glass N2 - This study suggests a tool for a better control on the sintering/crystallization of 3D-printed bioactive glassceramics bodies. A small cantilever in form of a bar with square cross section attached to a base and inclined 34◦ with the horizon, was used to monitor the viscous flow and sintering/crystallization headway of a glassceramic systems. 3D printing and sintering of bioactive glass-ceramics is of great interest for medical care applications. Viscous flow ensures sufficient densification of the typically low density printed green bodies, while crystallization prevents the structure from collapsing under the gravitational load. As a model system, a bioactive glass called BP1 (48.4 SiO2, 1 B2O3, 2 P2O5, 36.6 CaO, 6.6 K2O, 5.6 Na2O (mol%)), which has a chemical composition based on that of ICIE16, was employed in this work. In addition, ICIE16 was used as a reference glass. The results show that the suggested design is a very promising tool to track the real-time deformation of 3D printed glass-ceramic specimens and gives a good indication for the onset of crystallization as well. KW - Real-time deformation KW - Sintering KW - 3D-printing KW - Bioactive glass PY - 2021 DO - https://doi.org/10.1016/j.ceramint.2021.03.334 VL - 47 IS - 14 SP - 20045 EP - 20050 PB - Elsevier Ltd. AN - OPUS4-53449 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Schilling, Markus A1 - Bayerlein, Bernd A1 - Olbricht, Jürgen A1 - Skrotzki, Birgit T1 - Towards digitalization of materials in PMD: An application ontology of the tensile test N2 - Due to the diversity of materials and the processes associated with their production and use, the complexity of the lifecycles of materials and the multitude of academic and industrial researchers participating in generation of data for material design impose a huge challenge. The topical goal of digitalizing materials and processes can only be adequately addressed by consolidating the efforts of all stakeholders in this field. There are many scattered activities, but there is a demand for an elimination of redundancies as well as an advance in acceptance and a common basis in the digitalization of materials. Furthermore, data analysis methods play an important role in both, the experimental and simulation-based digital description of materials, but they have been poorly structured so far. Therefore, the two joint projects Platform Material Digital (PMD, materialdigital.de) and Materials open Laboratory (Mat-o-Lab, matolab.de) aim to contribute to a standardized description of data processing methods in materials research. Besides stimulating the formation of a collaborative community in this respect, their main technical goals are the quality assurance of the processes and the output data, the acquisition and definition of their accuracy as well as the interoperability between applications. In this regard, data management in accordance with the FAIR (findability, accessibility, interoperability, reuseability) principles is addressed. There is a common agreement in the scientific community following current discussions that data is supposed to be conform to these principles. This includes storage, processing and querying of data in a preferably standardized form. To meet the challenge to contextualize material data in a way that is consistent with all stakeholders, all necessary information on the condition of the material including production and application-related changes have to be made available via a uniform, machine-readable description. For this purpose, ontologies are to be used since they allow for machine-understandable knowledge representations and conceptualizations that are needed for data management and the digitalization in the field of materials science. As first efforts in PMD and Mat-o-Lab, application ontologies are created to explicitly describe processes and test methods. Thereby, the well-known tensile test of metals at room temperature was described ontologically in accordance with the respective ISO standard 6892-1:2019-11. The efforts in creating this tensile test application ontology are shown in this presentation. Especially, the path of ontology development based on standards to be pursued is focused, which is in accordance with the generic recommendations for ontology development and which is supposed to be exemplary for the creation of other application ontologies. T2 - VirtMet: 1st International Workshop on Metrology for Virtual Measuring Instruments and Digital Twins CY - Online meeting DA - 21.09.2021 KW - Platform Material Digital (PMD) KW - Ontology KW - Tensile test KW - Standard KW - Ontology development PY - 2021 AN - OPUS4-53481 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CHAP A1 - Fedelich, Bernard ED - Cailletaud, G. ED - Cormier, J. ED - Eggeler, G. ED - Maurel, V. ED - Nazé, L. T1 - Crystal orientation and elastic properties N2 - The elastic constants are the most basic mechanical properties of a material and are needed for any structural analysis of a component. For example, they have a major influence on the eigenfrequencies of vibrating parts. Single crystals of Ni-base superalloys are strongly anisotropic, which means that the observed properties are orientation dependent. Tensor algebra is then required to mathematically formulate the elastic properties and their relations to the crystal orientation. Hence, this chapter first summarizes some basic definitions and calculation rules for Rotation matrices, including the definition of the Euler angles, which are most commonly used to define the relative orientations of the crystal and the component. Parts of this chapter closely follow the lines of the excellent exposition of the topic by Olschewski. KW - Nickel-base superalloys KW - Elasticity PY - 2022 SN - 978-0-12-819357-0 SP - 41 EP - 67 PB - Elsevier Inc. AN - OPUS4-53435 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CHAP A1 - Fedelich, Bernard ED - Cailletaud, G. ED - Cormier, J. ED - Eggeler, G. ED - Maurel, V. ED - Nazé, L. T1 - Crystal plasticity models: dislocation based N2 - The large number of TEM investigations and the regular microstructure of single-crystal nickel-base superalloys has boosted the development of a number of physically motivated constitutive laws. In contrast to the more phenomenological models discussed in the next chapter, these models use dislocation densities as internal variables. Obvious advantages are that the computed densities can be compared to TEM observations and the Deformation mechanisms can be easier translated into mathematical equations. KW - Nickel-base superalloys KW - Creep KW - Plasticity PY - 2022 SN - 978-0-12-819357-0 SP - 401 EP - 427 PB - Elsevier Inc. ET - 1 AN - OPUS4-53436 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Thuy, Maximilian A1 - Niebergall, Ute A1 - Böhning, Martin T1 - Influence of molecular orientation on the environmental stress cracking resistance N2 - Molecular orientation has a significant effect on the material properties of polymers. Preferential orientation of the microstructure (polymer chains or crystallites) in a specific direction or plane often enhances the material properties, especially if the high-strength covalent bonds are primarily exposed to loads instead of the weaker van der Waals bonds. However, the orientation-dependent microstructure and its mechanical behavior is in general already well understood by many scientific studies [1-3]. Isotropic materials are frequently required for an intrinsic material characterization without prevailing processing-induced properties, as is the case for Full Notch Creep Test (FNCT) [4] addressing environmental stress cracking (ESC) in high-density polyethylene (PE-HD) [5, 6]. Since ESC is one of the major limiting issues for long-term performance of PE-HD pipes and containers [7], which in contrast have a production-related preferential orientated microstructure due to extrusion or extrusion blow molding, it is important to additionally investigate the ESC resistance of such anisotropic microstructure. Investigations of the slow crack growth (SCG) with respect to the molecular orientation generally obtain a factor of 1.2 up to 4.7 between crack growth perpendicular to the extrusion direction and crack growth parallel to the extrusion direction 8. Based on FNCT investigations with an aqueous detergent solution as environmental medium, hot pressed sheets with isotropic morphology are compared with extruded sheets from which specimens with different orientation angles are taken. However, the time to failure obtained by FNCT is also significantly influenced by the different cooling conditions under which the final morphology is formed. The tendency of the specimen to fail due to ESC is investigated as a function of environmental medium temperature. For a more detailed analysis of the affecting parameters in the manufacturing process, the ESC resistance is discussed considering the differences in crystallinity as revealed by thermal analysis. T2 - 36th International Conference of the Polymer Processing Society CY - Montreal, Canada DA - 26.09.2021 KW - Environmental stress cracking KW - Orientation-dependent microstructure KW - High-density polyethylene KW - Full Notch Creep Test PY - 2021 AN - OPUS4-53399 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Thuy, Maximilian A1 - Niebergall, Ute A1 - Böhning, Martin T1 - Damage progression of environmental stress cracking affected by manufacturing process-induced microstructural orientation N2 - Currently, the Full Notch Creep Test (FNCT) [1] method is used by material suppliers and end users in industry for the approval of container and pipe materials based on high-density polyethylene (PE-HD). The resistance to environmental stress cracking (ESC) of the material is evaluated using the time to failure of the specimen in an aqueous solution of a detergent [2, 3]. Usually specimens made of sheets with isotropic material properties, manufactured by hot pressing, are employed in order to obtain intrinsic properties of the material in terms of ESC failure. In contrast, the processes used in manufacturing to form containers and pipes, such as extrusion blow molding or extrusion, impose anisotropic properties to the material. These are mostly due to a microstructural orientation (polymer chains or crystallites) [4]. Furthermore, the different cooling conditions significantly affect the size distribution of crystallites as well as the overall morphology. It is therefore essential to understand the influence of process-induced material characteristics on failure due to ESC. A large number of studies on material properties as a function of microstructural preferential orientation have already been conducted [5-7]. However, effects on ESC as the major failure mechanism of containers and pipes are still rather unexplored [8, 9]. The most important factor is whether primarily intramolecular high-strength covalent bonds or the substantially weaker intermolecular van der Waals forces are predominantly loaded. In addition to the widely established classification by time to failure, the strain or crack opening displacement (COD) provides valuable information about the evolution and progression of damage as a function of time [10, 11]. Optical strain measurement using digital image correlation allows the differences in COD for isotropic and different angles of orientation of anisotropic specimens to be discussed. Also, a post-fracture surface analysis provides clarification on the craze-crack mechanism of the ESC. These different ESC-related properties of extruded and hot-pressed specimens have been investigated at different environmental medium temperatures and different initial stresses to provide a broad characterization of the fracture behavior of PE-HD. T2 - 36th International Conference of the Polymer Processing Society CY - Montreal, Canada DA - 26.09.2021 KW - Environmental stress cracking KW - High-density polyethylene KW - Fracture behavior KW - Microstructural orientation PY - 2021 AN - OPUS4-53400 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Schilling, Markus A1 - Niebergall, Ute A1 - Böhning, Martin T1 - Umgebungsinduzierte Spannungsrissbildung (ESC) von PE-HD induziert durch äußerliche Einwirkung organischer Flüssigkeiten N2 - Polyethylen hoher Dichte (PE-HD) wird als Werkstoff für Rohre und Behälter für den Transport und zur Lagerung von Gefahrgütern verwendet. Für die Beurteilung und technische Freigabe dieser Materialien ist insbesondere das Verständnis des Schädigungsmechanismus des langsamen, umgebungsbedingten Spannungsrisses (engl.: „environmental stress cracking“, ESC) essentiell. ESC tritt bei relativ geringen auf einen Werkstoff einwirkenden mechanischen Spannungen auf. An lokalen Fehlstellen (z.B. Defekte, Inhomogenitäten, Kerben) beginnend wächst ein Riss langsam durch das Material und führt nach gewisser Zeit zu einem charakteristischen, pseudo-spröden Bruch. Dabei wird das Risswachstum durch äußere Medieneinwirkung zusätzlich entscheidend beeinflusst. Dieses langsame Risswachstum wird als Hauptursache für das plötzliche und unerwartete Versagen von Polymerwerkstoffen angesehen. Eine etablierte Prüfmethode zur Bewertung des Materialverhaltens gegenüber dieses Schädigungsmechanismus ist der Full-Notch Creep Test (FNCT), der für PE-HD Behältermaterialien üblicherweise unter Verwendung von wässrigen Netzmittellösungen (Arkopal N 100) durchgeführt wird. Die aus dem FNCT erhaltene Standzeit dient dabei als Bewertungskriterium für verschiedene PE-HD-Werkstoffe. In einer Studie wurden neben einer typischen Arkopal-N-100-Netzmittellösung praktisch relevante, organische Flüssigkeiten wie Biodiesel und Diesel als Testmedien verwendet, um deren Einfluss auf das ESC-Verhalten von PE-HD-Behältermaterialien zu charakterisieren. Neben der klassischen Standzeit-Auswertung erfolgte eine erweiterte Bruchflächenanalyse mittels Licht- (LM), Laserscanning- (LSM) und Rasterelektronenmikroskopie (REM). Insbesondere die LSM erlaubt eine schnelle und einfache Unterscheidung pseudo-spröder und duktiler Bruchbilder, die zur Beurteilung der Repräsentativität des FNCT für das dem Spannungsriss zugrundeliegenden langsamen Risswachstum von Bedeutung ist. T2 - Polymer Service GmbH Merseburg - "Lebensdauerabschätzung von Polymerwerkstoffen - Möglichkeiten und Grenzen" CY - Merseburg, Germany DA - 27.03.2019 KW - Environmental Stress Cracking (ESC) KW - Slow Crack Growth (SCG) KW - Spannungsriss KW - Polyethylen hoher Dichte KW - Full-Notch Creep Test (FNCT) KW - Bruchflächenanalyse KW - Laserscanningmikroskopie (LSM) PY - 2019 AN - OPUS4-52947 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Agea Blanco, Boris A1 - Walzel, S. A1 - Chi, J. A1 - Lüchtenborg, J. T1 - Making Binder Jetting Really Work for Technical Ceramics - Additive Manufacturing of Technical Ceramics N2 - As an alternative shaping method to the traditionally used processes, additive manufacturing (AM) can produce economical ceramic components in small lot sizes and/or with complex geometries. Powder-based additive manufacturing processes like binder jetting are popular in the field of metal AM. One reason is the increased productivity compared to other AM technologies. For ceramic materials, powder-based AM technologies result in porous ceramic parts, provided they are not infiltrated. CerAMing GmbH unites the advantages of powder-based processes with the production of dense ceramic by means of the Layerwise Slurry Deposition. By using a suspension, a high packing density of the powder bed is achieved which leads to high green body densities. Due to this advantage the approach overcomes the problems of other powder-based AM technologies. Furthermore, a very economical debinding time allows the production of parts with high wall thicknesses. KW - Additive Manufacturing KW - Binder Jetting KW - Layerwise Slurry Deposition KW - Lithography-based technologies KW - Technical Ceramics PY - 2021 SP - 49 EP - 52 PB - Göller Verlag CY - Baden-Baden AN - OPUS4-52948 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Schilling, Markus T1 - Tensile Test Ontology used in Platform Material Digital (PMD) N2 - Data analysis methods play an important role in both the experimental and simulation-based digital description of materials but have so far been poorly structured. The platform Material Digital (PMD) is supposed to contribute to a standardized description of data processing methods in materials research. The goal is the quality assurance of the processes and the output data, the acquisition and definition of their accuracy as well as the interoperability between applications. Therefore, application ontologies are created to explicitly describe processes and test methods. In this presentation, the first efforts within the joint project PMD in creating a tensile test application ontology in accordance with the ISO standard 6892-1:2019-11 are shown. Especially, the path of ontology development to be pursued based on standards was focused. Furthermore, the presentation includes a live demonstration of queries possibly performed to query data that was uploaded in the PMD triple store. T2 - Online Workshop: An introduction to the semantic web and ontologies CY - Online meeting DA - 23.04.2021 KW - Ontology KW - Tensile Test KW - Platform Material Digital KW - PMD KW - Knowledge Graphs KW - Semantic Web PY - 2021 AN - OPUS4-52949 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Hildebrand, G. A1 - Sänger, Johanna Christiane A1 - Schirmer, U. A1 - Mantei, W. A1 - Dupuis, Y. A1 - Houbertz, R. A1 - Liefeith, K. T1 - Process Development for Additive Manufacturing of Alumina Toughened Zirconia for 3D Structures by Means of Two-Photon Absorption Technique N2 - Additive manufacturing is well established for plastics and metals, and it gets more and more implemented in a variety of industrial processes. Beside these well-established material platforms, additive manufacturing processes are highly interesting for ceramics, especially regarding resource conservation and for the production of complex three-dimensional shapes and structures with specific feature sizes in the µm and mm range with high accuracy. The usage of ceramics in 3D printing is, however, just at the beginning of a technical implementation in a continuously and fast rising field of research and development. The flexible fabrication of highly complex and precise 3D structures by means of light-induced photopolymerization that are difficult to realize using traditional ceramic fabrication methods such as casting and machining is of high importance. Generally, slurry-based ceramic 3D printing technologies involve liquid or semi-liquid polymeric systems dispersed with ceramic particles as feedstock (inks or pastes), depending on the solid loading and viscosity of the system. This paper includes all types of photo-curable polymer-ceramic-mixtures (feedstock), while demonstrating our own work on 3D printed alumina toughened zirconia based ceramic slurries with light induced polymerization on the basis of two-photon absorption (TPA) for the first time. As a proven exemplary on cuboids with varying edge length and double pyramids in the µm-range we state that real 3D micro-stereolithographic fabrication of ceramic products will be generally possible in the near future by means of TPA. This technology enables the fabrication of 3D structures with high accuracy in comparison to ceramic technologies that apply single-photon excitation. In sum, our work is intended to contribute to the fundamental development of this technology for the representation of oxide-ceramic components (proof-of-principle) and helps to exploit the high potential of additive processes in the field of bio-ceramics in the medium to long-term future. KW - Additive manufacturing KW - Ceramics 3D printing KW - Two-photon adsorption KW - Polymer-ceramic mixtures KW - Bio-ceramic engineering PY - 2021 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-526672 DO - https://doi.org/10.3390/ceramics4020017 VL - 4 IS - 2 SP - 224 EP - 239 PB - MDPI CY - Basel AN - OPUS4-52667 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Abboud, M. A1 - Motallebzadeh, A. A1 - Duygulu, O. A1 - Maaß, Robert A1 - Özerinc, S. T1 - Microstructure and nanomechanical behavior of sputtered CuNb thin films N2 - We report on the mechanical properties of Cu–Nb alloys produced by combinatorial magnetron sputtering. Depending on the composition, the microstructure is either fully amorphous (~30–65 at.% Cu), a dispersion of Cu crystallites in an amorphous matrix (~70 at.%), or a dominant crystalline phase with separated nanoscale amorphous zones (~80 at.% Cu). Nanomechanical probing of the different microstructures reveals that the hardness of the fully amorphous alloy is much higher than a rule of mixture would predict. We further demonstrate a remarkable tunability of the resistance to plastic flow, ranging from ca. 9 GPa in the amorphous regime to ca. 2 GPa in the fully crystalline regime. We rationalize these findings based on fundamental structural considerations, thereby highlighting the vast structure-property design space that this otherwise immiscible binary alloy provides. KW - Deposition microstructure KW - Metallic glasses KW - Thin films KW - Mechanical properties KW - Nanocrystalline structure PY - 2021 DO - https://doi.org/10.1016/j.intermet.2021.107249 SN - 0966-9795 VL - 136 SP - 1 EP - 7 PB - Elsevier CY - Amsterdam AN - OPUS4-52777 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Rabe, Torsten A1 - Eichler, J. A1 - Picht, G. A1 - Rossner, W. A1 - Stelter, M. A1 - Voigt, I. T1 - Digitalisierung der keramischen Fertigung - Herausforderungen und Chancen N2 - Dieses Strategiepapier zielt darauf ab, Akteuren und Entscheidungsträgern den Status der Digitalisierung in der keramischen Fertigung, erfolgreiche Best-Practice-Beispiele aber auch die Herausforderungen nahezubringen, die es nun anzugehen gilt. Es ist die Vision, die Keramikfertigung durchgehend zu digitalisieren und alle Schritte des Produktkreislaufs lückenlos über die gesamte Wertschöpfungs- und Nutzungskette zu vernetzen: also eine Keramikindustrie 4.0 zu etablieren. Das Strategiepapier erfasst zunächst die Spezifität der keramischen Fertigung und nimmt eine Analyse des gegenwärtigen Standes der Digitalisierung in der keramischen Industrie vor, auch anhand einiger ausgewählter Beispiele aus der industriellen Praxis. Auf Basis der wesentlichen Bausteine für eine Fertigungsdigitalisierung werden schließlich die Chancen für Keramikproduzenten sowie der erforderliche Forschungs- und Entwicklungsbedarf aufgezeigt. KW - Datenmanagement KW - Digitalisierung KW - Fertigungsprozess KW - Keramik KW - Sensorik PY - 2021 SP - 1 EP - 39 PB - Deutsche Gesellschaft für Materialkunde (DGM) und Deutsche Keramische Gesellschaft (DKG) CY - Köln ET - 1000 AN - OPUS4-52708 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Gebhardt, M. A1 - Manolakis, I. A1 - Chatterjee, A. A1 - Kalinka, Gerhard A1 - Deubener, J. A1 - Pfnür, H. A1 - Chakraborty, S. A1 - Meiners, D. T1 - Reducing the raw material usage for room temperature infusible and polymerisable thermoplastic CFRPs through reuse of recycled waste matrix material N2 - In this work, a closed loop recycling process is investigated, which allows polymerised bulk thermoplastic matrix (Elium 150) from production waste (also referred to as recyclate) to be reused as additive in composite manufacturing by vacuum assisted resin infusion (VARI) of virgin Elium 150 monomer. It is shown that this process can save up to 7.5 wt% of virgin material usage in each processing cycle. At the same time, the thermal stability and stiffness of the composite increases with the proportion of recyclate introduced. Contemporarily, the shear and bending properties have also been observed to improve. Gel permeation chromatography (GPC) showed that the changes observed are due to an increase in molecular weight with the recyclate content. In particular, a correlation between the molecular weight and the shear properties of the composite was discovered using single fibre push-out tests. KW - Mechanical properties KW - Recycling KW - Carbon fibres KW - Fibre/matrix bond PY - 2021 DO - https://doi.org/10.1016/j.compositesb.2021.108877 SN - 1359-8368 VL - 216 SP - 108877 PB - Elsevier Ltd. CY - Niederlande AN - OPUS4-52711 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Aristia, Gabriela A1 - Bäßler, Ralph A1 - Nofz, Marianne A1 - Sojref, Regine A1 - Kohl, Anka T1 - Short-term exposure tests of ɣ-Al2O3 Sol-gel coating on X20Cr13 in artificial geothermal waters with different pH N2 - The suitability of an Al2O3 coating for corrosion protection on X20Cr13 was evaluated in various artificial geothermal brines, focusing on the influence of different pH (4, 6 and 8) and their chemical compositions on the coating properties. All experiments were performed in the laboratory using autoclaves at 150 ◦C and 1 MPa in deaerated condition for 1 and 7 days. Results showed that the pH of geothermal waters is the most detrimental factor in the transformation of ɣ-Al2O3 and its protective abilities. Delaminations were found in the Coating exposed to geothermal brines with pH 4. FTIR spectra indicated a transformation of ɣ-Al2O3 to boehmite AlOOH after exposure to pH 4 and 6, and bayerite Al(OH)3 was formed after exposure to pH 8. Different Crystal structures of the hydrated Al2O3 also contribute to the stability of the coatings, observed by the SEM- EDX of the surface and cross-section of coatings. This study indicated that ɣ-Al2O3 sol-gel coating presents a promising aspect of corrosion protection in geothermal environment with a neutral pH. KW - Al2O3 KW - Corrosion KW - Coating KW - Martensitic steel PY - 2021 DO - https://doi.org/10.1016/j.geothermics.2021.102193 SN - 0375-6505 VL - 96 SP - 102193 PB - Elsevier Ltd. CY - Amsterdam AN - OPUS4-52931 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Waurischk, Tina A1 - Reinsch, Stefan A1 - Rouxel, T. A1 - Behrens, H. A1 - Deubener, J. A1 - Müller, Ralf T1 - Vacuum crack growth in alkali silicate glasses N2 - Crack growth velocity in alkali silicate glasses was measured in vacuum across 10 orders of magnitude with double cantilever beam technique. Measured and literature crack growth data were compared with calculated intrinsic fracture toughness data obtained from Young´s moduli and the theoretical fracture surface energy estimated from chemical bond energies. Data analysis reveals significant deviations from this intrinsic brittle fracture behavior. These deviations do not follow simple compositional trends. Two opposing processes may explain this finding: a decrease in the apparent fracture surface energy due to stress-induced chemical changes at the crack tip and its increase due to energy dissipation during fracture. KW - Silicate glass KW - Brittle fracture KW - Crack growth KW - Calculated intrinsic fracture toughness PY - 2021 DO - https://doi.org/10.1016/j.jnoncrysol.2021.121094 SN - 0022-3093 VL - 572 SP - 1 EP - 8 PB - Elsevier CY - Amsterdam AN - OPUS4-53144 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Baesso, Ilaria A1 - Karl, D. A1 - Spitzer, Andrea A1 - Gurlo, A. A1 - Günster, Jens A1 - Zocca, Andrea T1 - Characterization of powder flow behavior for additive manufacturing N2 - The flow behavior of powders has an essential role in many industrial processes, including powder bed additive manufacturing. The characterization of the flow behavior is challenging, as different methods are available, and their suitability for an application in additive manufacturing is still controversial. In this study, six standardized methods (measurement of bulk density by ISO 60 and by ASTM B329, angle of repose by ISO 4324, discharge time by ISO 6186 and by ASTM B964-16, and Hausner Ratio by ASTM 7481 – 18), the rotating drum method (by GranuDrum) and powder rheometry (Anton Paar powder cell), were applied to five size fractions of a crushed quartz sand powder and compared. A statistical approach is proposed and discussed to correlate the obtained flowability indexes with the packing density of powder beds deposited layer-by-layer, and these correlations are compared between methods. Overall, the measurement of bulk density by ASTM B329 that showed the best correlation with the powder bed density. Advanced methods such as the rotating drum method and powder rheometry did not demonstrate particularly good correlations, however they provided complementary information which can be useful to assess the dynamic behavior of powders. KW - Powder flow KW - Flowability KW - Powder bed additive manufacturing KW - Powder rheology PY - 2021 DO - https://doi.org/10.1016/j.addma.2021.102250 SN - 2214-8604 VL - 47 SP - 1 EP - 14 PB - Elsevier CY - Amsterdam AN - OPUS4-53229 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Abram, Sarah-Luise A1 - Mrkwitschka, Paul A1 - Prinz, Carsten A1 - Rühle, Bastian A1 - Haase, Oskar A1 - Kuchenbecker, Petra A1 - Löhmann, Oliver A1 - Hodoroaba, Vasile-Dan A1 - Bresch, Harald A1 - Resch-Genger, Ute T1 - Iron oxide nanoparticles as a reference material candidate for particle size measurements N2 - This poster presentation covers the development of iron oxide nanoparticles as reference material candidate in the context of the project "Nanoplattform". T2 - EMRS Spring Meeting CY - Online meeting DA - 31.05.2021 KW - Iron oxide nanoparticles KW - Reference material KW - Particle size KW - Transmission electron microscopy KW - Small angle x-ray scattering PY - 2021 AN - OPUS4-52773 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Abram, Sarah-Luise A1 - Mrkwitschka, Paul A1 - Prinz, Carsten A1 - Rühle, Bastian A1 - Kuchenbecker, Petra A1 - Hodoroaba, Vasile-Dan A1 - Resch-Genger, Ute T1 - Monodisperse iron oxide nanoparticles as reference material candidate for particle size measurements N2 - In order to utilize and rationally design materials at the nanoscale the reliable characterization of their physico-chemical properties is highly important, especially with respect to the assessment of their environmental or biological impact. Furthermore, the European Commission’s REACH Regulations require the registration of nanomaterials traded in quantities of at least 1 ton. Powders or dispersions where 50% (number distribution) of the constituent particles have sizes ≤ 100 nm in at least one dimension are defined as nanomaterials. This creates a need for industrial manufacturers and research or analytical service facilities to reliably characterize potential nanomaterials. Currently, BAM is developing reference nanoparticles, which shall expand the scarce list of worldwide available nano reference materials certified for particle size distribution and will also target other key parameters like shape, structure, porosity or functional properties. In this respect, materials like iron oxide or titanium dioxide are considered as candidates to complement the already available silica, Au, Ag, and polystyrene reference nanoparticles. The thermal decomposition of iron oleate precursors in high boiling organic solvents can provide large quantities of iron oxide nanoparticles that can be varied in size and shape.[1, 2] The presence of oleic acid or other hydrophobic ligands as capping agents ensures stable dispersion in nonpolar solvents. Such monodisperse, spherical particles were synthesized at BAM and pre-characterized by electron microscopy (TEM, SEM including the transmission mode STEM-in-SEM) and dynamic light scattering comparing cumulants analysis and frequency power spectrum. 1. REACH regulations and nanosafety concerns create a strong need for nano reference materials with diverse properties. 2. Iron oxide nanoparticles are under development as new candidate reference material at BAM. 3. Narrow particle size distribution confirmed by light scattering and electron microscopy. T2 - Nanosafety 2020 CY - Online meeting DA - 05.10.2020 KW - Iron oxide nanoparticles KW - Reference material KW - Particle size KW - Electron microscopy KW - Nanoplattform PY - 2020 AN - OPUS4-52774 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Ghafafian, Carineh A1 - Trappe, Volker T1 - The effect of fiber orientation mismatch on scarf joint damage mechanisms under fatigue load N2 - Wind turbine rotor blades commonly fail before their projected 20-year lifespan largely due to defects that originate during manufacturing and are propagated by operational fatigue and environmental conditions. The cost-intensive replacement outcomes lead to a high loss of earnings, and are one of the inhibitors of wind turbine production. A potential repair alternative to restoring the mechanical properties of such lightweight fiber reinforced polymer (FRP) structures is to locally patch these areas with scarf joints. This type of repair allows for a smoother load distribution across the joint, and is favored especially on structures where minor aerodynamic contour changes are key. The effects of such repairs on the structural integrity, however, is still largely unknown. Building upon an understanding of the static load failure mechanism of GFRP scarf joints, presented at the ICCS23 Joint Event in 2020, the influence of the fiber orientation mismatch between parent and repair materials of 1:50 scarf joints on the failure mechanism of monolithic glass FRP specimens under cyclic fatigue load were examined in this study. Specimens with various layups were produced with the vacuum-assisted resin infusion (VARI) process using biaxial E-glass non-crimp fabric (NCF). The patch layers were then joined directly to the parent structure with the VARI using biaxial E-glass NCF with half the areal weight of the parent side to allow for better drapability. This mimics the soft-to-hard patch style utilized in wind turbine blade shell field repairs. The specimens were tested under uniaxial fatigue load, during which they were periodically monitored for damage onset. A comparison of the +45/-45° and 0/90° layups allowed for an understanding of the role of a highly mismatching fiber orientation in the transition zone between parent and patch material on the failure mechanism of the scarf joint. In addition to the tensile strength and stiffness property recovery assessment, a grayscale analysis using in-situ camera images determined the damage state leading to failure in each region across the scarf joint, which varied in the parent material versus scarf joint region, providing insight to the critical regions in this composite structure under cyclic loading. T2 - ICCS24 - 24th International Conference on Composite Structures CY - Online meeting DA - 14.06.2021 KW - Glass fiber reinforced polymers KW - Scarf repairs KW - Damage mechanisms PY - 2021 AN - OPUS4-52817 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Heuser, Lina A1 - Schmid, Thomas A1 - Deubener, J. T1 - An overview of structural, physical and thermal properties of low melting zinc and lead borate glasses N2 - Low melting zinc borate glasses awake interest to replace lead borate glasses in the silver metallization pastes for solar cells or microelectronics. In the current study, characteristic properties of alkali zinc borate glasses (X2O-ZnO-B2O3, X = Li, Na, K, Rb) were compared to an earth alkali zinc borate glass (CaO-ZnO-B2O3). Additionally, zinc oxide is partially substituted by lead oxide or cooper oxide in the borate glasses (Li2O-PbO-B2O3, Na2O ZnO CuO-B2O3). The alkali zinc borate glasses indicate less differences in Raman spectra, and thus in structural properties, in comparison to the Ca and Pb ions influence. LPbB (Tg = 401 °C) has a lower viscosity than LZB (Tg = 468 °C) and CaZB has the highest glass transition temperature (Tg = 580 °C). The Angell plot for the alkali zinc borate glasses shows a high fragility m = 80. Besides Tg, the density measured by means of the Archimedean principle, molar volume, and coefficient of thermal expansion (CTE) of the glasses were investigated. Trends could be found according to alkali ions or intermediate oxides. The density increases with decreasing alkali ion size from KZB (2.632 g/cm3) to LZB (2.829 g/cm3) and increases from LZB to LPbB (3.764 g/cm3). CTE ranges between 7.09 10-6 K-1 for CaZB and 11.5 10 6 K 1 for KZB and RZB. The differential thermal analysis (DTA) and X ray diffraction (XRD) indicate crystallization of various crystalline phases during heating with 5 K/min in most cases. T2 - 94. Glastechnische Tagung CY - Online meeting DA - 10.05.2021 KW - Borate glasses KW - Glass structure KW - Viscosity KW - Young´s Modulus KW - Alkali ions PY - 2021 AN - OPUS4-52867 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Heuser, Lina A1 - Sobek, P. A1 - Körner, S. A1 - Müller, Ralf T1 - Silver - alkali borate glass pastes N2 - Network modifier ions can decisively influence properties and structure of low melting alkali-zinc-borate glasses and thus cause complex effects on the liquid phase sintering of silver-glass metallization pastes. This effect was studied for X2O-ZnO-B2O3 (X = Li, Na, Rb) glasses for silver-glass metallization pastes. Viscosity and the glass transition temperature, Tg, were measured with rotational viscometry and dilatometry. Dried model pastes with 30 vol% LZB, NZB or RZB glass were prepared for sintering studies by means of heating microscopy measuring the silhouette area shrinkage of uniaxially pressed powder compacts during heating at 5 K/min. For comparison, the silhouette area shrinkage of pure glass and silver powder compacts were determined. Glass-silver wetting was investigated during heating of bulk glass cylinders placed on silver substrates. Glass RZB turned out to have the lowest viscosity among the glasses under study. Its glass transformation temperature, Tg, was found at 444 °C and it caused the lowest sintering onset for its glass and paste powder compacts. Slightly increased values of Tg were found for NZB and LZB (468 °C and 466 °C, respectively) and a slightly retarded sintering was found for both paste powder compacts. These results indicate that liquid phase sintering of silver-glass pastes under air atmosphere is mainly influenced by glass viscosity. T2 - GLASS MEETING 2020 CY - Online meeting DA - 07.12.2020 KW - Silver-glass metallization paste KW - Sintering KW - Alkali ions KW - Viscosity KW - Silver precipitates PY - 2020 AN - OPUS4-52871 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bresch, Sophie T1 - Entwicklung thermoelektrischer Multilayergeneratoren auf der Basis von Calciumcobaltit N2 - Thermoelectric generators can be used as energy harvesters for sensor applications. Multilayer thermoelectric generators (ML-TEGs) are a promising alternative to conventional π-type generators due to their high filling factor, high capability of automated production and the texturing potential during the production process. Calcium cobaltite is a promising thermoelectric oxide (p-type) with highly anisotropic properties. The following study shows the development of a textured unileg ML-TEG using ceramic multilayer technology. Tape-casting and pressure assisted sintering are applied to fabricate textured calcium cobaltite. Compared to conventional sintering, pressure assisted sintering increases the strength by the factor 10. Thermoelectric properties can be tuned either towards maximum power factor or towards maximum figure of merit depending on the pressure level. As electrical insulation material, a screen-printable glass-ceramic with high resistivity and adapted coefficient of thermal expansion is developed. From various commercial pastes a metallization with low contact resistance is chosen. The unileg ML-TEG is co-fired in one single step. The demonstrators reach 80% of the simulated output power and the power output is highly reproducible between the different demonstrators (99%). These results provide the first proof-of-concept for fabricating co-fired multilayer generators based on textured calcium cobaltite with high power factor, high density, and high strength. N2 - Thermoelektrische Generatoren können zum „Energy harvesting“ für den autarken Betrieb von bspw. Sensoren eingesetzt werden. Eine interessante Alternative zu den herkömmlichen π-Typ Generatoren sind auf Grund der höheren Leistungsdichte und der guten Automatisierbarkeit thermoelektrische Multilayergeneratoren. Calciumcobaltit ist ein vielsprechendes oxidisches Thermoelektrika (p-Typ) mit stark anisotropen Eigenschaften. Die hier vorgestellte Studie zeigt die Entwicklung von texturierten Unileg-Multilayer-Generatoren mittels keramischer Multilayertechnologie. Calciumcobaltit wird durch Foliengießen und druckunterstützte Sinterung texturiert. Im Vergleich zur konventionellen Sinterung verbessert sich die Festigkeit um den Faktor 10. Die thermoelektrischen Eigenschaften können je nach verwendetem Druckniveau hinsichtlich maximalem Power Factor oder hinsichtlich maximalem Gütefaktor optimiert werden. Ein Glaskeramikkomposit wird als Isolationsmaterial mit hohem Volumenwiderstand und angepasstem Wärmeausdehnungskoeffizienten entwickelt. Der Unileg-Multilayer-Generator wird in einem Schritt co-gesintert. Die hergestellten Demonstratoren erreichen 80% der simulierten Output-Leistung. Diese Ergebnisse stellen den ersten Machbarkeitsnachweis für die Herstellung von co-gesinterten Multilayer-Generatoren aus texturiertem Calciumcobaltit mit hohem Power Factor und hoher Festigkeit dar. T2 - Seminar des Lehrstuhls für Funktionsmaterialien, Universität Bayreuth CY - Online meeting DA - 18.06.2021 KW - Thermoelektrischer Generator KW - Multilayertechnik KW - Energy harvesting PY - 2021 AN - OPUS4-52834 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Kraus, David A1 - Trappe, Volker T1 - Transverse damage in glass fiber reinforced polymer under thermo-mechanical loading N2 - In this study, the thermomechanical damage behavior of a glass fiber reinforced polymer material is investigated. The coefficients of thermal expansion of the composite as well as the matrix are measured in a wide temperature range. Quasi-static experiments with neat resin, unidirectional and multidirectional laminates are performed as well as fatigue experiments in a temperature range from 213 K to 343 K. This study focusses on the matrix damage due to fiber-parallel loading. A correlation between matrix effort, the dilatational strain energy of the matrix and the damage state of the specimen is demonstrated. It is shown that a fatigue life assessment can be performed with the aid of a temperature-independent master fatigue curve. KW - Composite KW - Glass fiber reinforced polymer KW - Thermo-mechanics KW - Fatigue KW - Damage KW - Temperature PY - 2021 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-527462 DO - https://doi.org/10.1016/j.jcomc.2021.100147 SN - 2666-6820 VL - 5 SP - 100147 PB - Elsevier B.V. AN - OPUS4-52746 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Höhne, Patrick A1 - Rabe, Torsten T1 - Limits of computer tomography aided characterization of different types of porous ceramic materials N2 - Ceramics with open porosity are attractive materials in many fields of applications covering medicine, catalysis, and filtration. Manifold technologies to produce porous ceramics are available, e.g. foaming and replica processes, resulting in various microstructures. Development and manufacturing of new materials is accelerating, while crucial characterization is becoming increasingly difficult and conventional measurements lack the desired speed. Computed tomography (CT) offers the possibility to three-dimensionally characterize entire samples with minimal sample preparation, while its main advantage is that it is non-destructive. Still, the assessment of quantitative results from CT measurements is not trivial. The poster presents CT characterizations of newly developed as well as commercially available openly porous ceramic samples. Properties such as porosity, permeability or pore characteristics were measured conventionally and compared to results calculated from CT-measurements using the commercial software VG StudioMax. The determined differences between measured and calculated values are presented and application areas as well as limits of the CT characterization are evaluated. T2 - Jahrestagung der Deutschen keramischen Gesellschaft 2021 CY - Online Meeting DA - 19.04.2021 KW - Ceramic KW - Porosity PY - 2021 AN - OPUS4-52724 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Charmi, Amir T1 - Mechanical anisotropy of LPBF 316L: a modeling approach N2 - The underlying cause of mechanical anisotropy in additively manufactured (AM) parts is not yet fully understood and has been attributed to several different factors like microstructural defects, residual stresses, melt pool boundaries, crystallographic and morphological textures. To better understand the main contributing factor to the mechanical anisotropy of AM stainless steel 316L, bulk specimens were fabricated via laser powder bed fusion (LPBF). Tensile specimens were machined from these AM bulk materials for three different inclinations relative to the build plate. Dynamic Young's modulus measurements and tensile tests were used to determine the mechanical anisotropy. Some tensile specimens were also subjected to residual stress measurement via neutron diffraction, porosity determination with X-ray micro-computed tomography, and texture analysis with electron backscatter diffraction (EBSD). A crystal plasticity model was used to analyze the elastic anisotropy and the anisotropic yield behavior of the AM specimens, and it was able to capture and predict the experimental behavior accurately. Overall, it was shown that the mechanical anisotropy of the tested specimens was mainly influenced by the crystallographic texture. T2 - 2. Online-Workshop "In-situ Monitoring and Microstructure Development in Additive Manufactured Alloys " CY - Online meeting DA - 20.04.2021 KW - Anisotropy KW - Crystal plasticity KW - Additive manufacturing PY - 2021 AN - OPUS4-52603 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Ávila Calderón, Luis Alexander T1 - Creep behavior and microstructural evolution of LPBF 316L N2 - This presentation shows some experimental results of the characterization of the creep behavior of LPBF 316L, which has been poorly studied and understood to date. The presentation includes results regarding the mechanical properties, the initial microstructural state and its evolution under loading, and the damage mechanism. This work was done within the BAM focus area materials project AGIL. As a benchmark to assess the material properties of the LPBF 316L, a conventionally manufactured variant was also tested. T2 - 2nd Workshop on In-situ Monitoring and Microstructure Development in Additive Manufactured alloys at BAM CY - Online Meeting DA - 19.04.2021 KW - 316L KW - Additive Manufacturing KW - Creep behavior PY - 2021 AN - OPUS4-52682 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Epishin, A. A1 - Camin, B. A1 - Hansen, L. A1 - Heuser, M. A1 - Lopez-Galilea, I. A1 - Ruttert, B. A1 - Theisen, W. A1 - Fedelich, Bernard T1 - Refinement and Experimental Validation of a Vacancy Model of Pore Annihilation in Single-Crystal Nickel-Base Superalloys during Hot Isostatic Pressing N2 - Initially, as-cast and homogenized single crystals of nickel-base superalloy CMSX-4 are subjected to hot isostatic pressing at 1288 °C. Two series of experiments are conducted: under the same pressure of 103 MPa but with different durations, between 0.5 and 6 h, and under different pressures, between 15 and 150 MPa, but for the same time of 0.5 h. The porosity annihilation is investigated metallographically and by high-resolution synchrotron X-ray tomography. The obtained experimental results are compared with the predictions of the vacancy model proposed recently in the group. Herein, the model is further refined by coupling with X-ray tomography. The model describes the evolution of the pore arrays enclosed in the 3D synchrotron tomograms during hot isostatic pressing and properly predicts the time and stress dependences of the pore annihilation kinetics. The validated model and the obtained experimental results are used for selecting the optimal technological parameters such as applied pressure and processing time KW - Superalloys KW - HIP KW - Single-Crystal KW - Diffusion PY - 2021 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-526859 DO - https://doi.org/10.1002/adem.202100211 VL - 23 IS - 7 SP - 211 AN - OPUS4-52685 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Thuy, Maximilian A1 - Niebergall, Ute A1 - Oehler, H. A1 - Alig, I. A1 - Böhning, Martin T1 - Evaluation of the damaging effect of crop protection formulations on high density polyethylene using the Full Notch Creep Test N2 - Four typical high-density polyethylene container materials were used to investigate damage or stress cracking behavior in contact with model liquids for crop protection products. These model liquids are established in German regulations for the approval of dangerous goods containers and consist of typical admixtures used for crop protection products but without biological active ingredients. This study is performed with the standardized method of Full Notch Creep Test, adapting the media temperature to 40 °C according to the usual conditions where these test liquids are applied. The two model liquids differ into a water-based solution and a composition based on different organic solvents which are absorbed by the material up to significant levels. Therefore, extensive sorption measurements are performed. The fracture surfaces obtained are analyzed in detail not only by light microscopy, but also by laser scanning microscopy as well as scanning electron microscopy. Influence of pre-saturation and applied stress are addressed by respective systematic series of experiments. KW - Polyethylene KW - Full Notch Creep Test KW - Environmental Stress Cracking KW - Fracture PY - 2021 DO - https://doi.org/10.1016/j.polymer.2021.123853 SN - 0032-3861 VL - 228 SP - 123853 PB - Elsevier Ltd. AN - OPUS4-52686 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Ghafafian, Carineh A1 - Trappe, Volker T1 - Restoring lightweight strength - Effect of localized repairs on the mechanical properties of composites sandwich structures N2 - As a type of high-performance composite material, glass-fiber reinforced plastics (GFRP) are favored for the construction of wind turbine rotor blades due to their high specific strength and stiffness properties (Grasse et al, 2010). During the blade manufacturing process, however, imperfections are often introduced, then further propagated due to harsh environmental conditions and a variety of loads (Caminero et al, 2013; Trappe et al, 2018). This leads to failure significantly before their designed lifespan. Since replacement of entire blades can be a costly potential outcome, localized repairs of the damaged region to restore structural integrity and thus lengthen its lifespan can executed in the field by technicians accessing the blades directly by suspended roping. These methods involve replacing the lost load path with a new material that is joined to the parent structure. In recent years, considerable studies have been conducted to investigate the influence of different repair parameters on the stress distribution, ultimate strength, impact behavior, and residual stresses of bonded repaired structures [Caminero et al, 2013; Trappe et al, 2018; Shufeng et al, 2014; Harman and Rider, 2011; Ahn and Springer, 2000; Lekou and Vionis, 2002). However, there currently do not exist any standardized repair procedures for wind turbine rotor blades. Namely, there is a lack of understanding about the effects of the layup of various repair methods, especially on the damage mechanism and fatigue life of the shells of rotor blades (Caminero et al, 2013; Trappe et al, 2018). This work therefore aims to begin to enrich this knowledge gap by testing the influence of different variables among repair patches on the mechanical properties of sandwich composite structures. Manufactured with the vacuum-assisted resin infusion (VARI) process, the test specimens are produced as a GFRP structure to represent the outer shell portion of a wind turbine blade, then repaired with a scarf joint. Scarf repairs are favored as the most efficient of the common structural joints, as the removal of the damaged area with angled walls leads to a nearly uniform shear stress distribution along the bond surface and no eccentricity in the load distribution (Caminero et al, 2013; Lekou and Vionis, 2002; Siener, 1992). The performance of specific layup methods of repair patches, namely a large-to-small versus small-to-large scheme of repair layers, is studied with static and load-controlled fatigue testing, then compared to pristine test specimens as well as to each other in terms of mechanical property restoration. The transition layer between repair and parent material is especially of interest in the performance of the structure. Damage onset, crack development and eventual failure are monitored in-situ with non-destructive testing methods, including thermography with an infrared camera system and a 3D deformation analysis system, to develop a more robust understanding of the effects of these repair concept variables on wind turbine blade shell structures. T2 - Wind Energy Science Conference CY - Online Meeting DA - 25.05.2021 KW - Glass fiber reinforced polymers KW - Wind turbine blade shell structures KW - Scarf joint repair PY - 2021 AN - OPUS4-52687 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Mrkwitschka, Paul A1 - Kuchenbecker, Petra A1 - Hodoroaba, Vasile-Dan A1 - Rabe, Torsten T1 - Comparative study of suitable preparation methods to evaluate irregular shaped, polydisperse nanoparticles by scanning electron microscopy (SEM). N2 - Reliable characterization of materials at the nanoscale regarding their physio-chemical properties is a challenging task, which is important when utilizing and designing nanoscale materials. Nanoscale materials pose a potential toxicological hazard to the environment and the human body. For this reason, the European Commission amended the REACH Regulation in 2018 to govern the classification of nanomaterials, relying on number-based distribution of the particle size. Suitable methods exist for the granulometric characterization of monodisperse and ideally shaped nanoparticles. However, the evaluation of commercially available nanoscale powders is problematic. These powders tend to agglomerate, show a wide particle size distribution and are of irregular particle shape. Zinc oxide, aluminum oxide and cerium oxide with particle sizes less than 100 nm were selected for the studies and different preparation methods were used comparatively. First, the nanoparticles were dispersed in different dispersants and prepared on TEM-supported copper grids. Furthermore, individual powders were deposited on carbon-based self-adhesive pads. In addition, the samples were embedded by hot mounting and then ground and polished. The prepared samples were investigated by scanning electron microscopy (including the transmission mode STEM-in-SEM) and Dynamic Light scattering. The software package ImageJ was used to segment the SEM images and obtain the particle sizes and shapes and finally the number-based particles size distribution with size expressed as various descriptors. T2 - Ceramics 2021 CY - Online meeting DA - 19.04.2021 KW - Nanoparticles KW - Preparation KW - Characterization PY - 2021 AN - OPUS4-53272 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Meyer, Lena A1 - Günster, Jens T1 - Powder based Additive Manufacturing in Space N2 - Abstract of the event: 'The area of New Space is a vastly growing and dynamic field with a high innovative potential and many exciting ideas. After decades where activities in space were dominated and funded mainly by governmental agencies, a new industry is forming and new business models are being developed around ideas like satellite-based internet, space travel, space mining, geo-monitoring etc. For space applications, lightweight design is crucial to keep the costs at a minimum. This Innovation Day will introduce the field of New Space and present the variety of exciting opportunities that arise for composites based on their excellent lightweight potential.' Another research area is now arising in the field of 3D printing or additive manufacturing of fiber composite materials in space. At the event, we presented on the opportunities and our experiences of using a powder based additive manufacturing process for in-space manufacturing applications. T2 - CU Innovation Day - New opportunities and applications in space with composites CY - Online meeting DA - 29.03.2022 KW - μ-gravity KW - In-space manufacturing KW - Additive manufacturing KW - Microgravity KW - Powder PY - 2022 AN - OPUS4-54559 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Chen, Yue A1 - Schilling, Markus A1 - von Hartrott, P. A1 - Huschka, M. A1 - Olbricht, Jürgen A1 - Pirskawetz, Stephan A1 - Skrotzki, Birgit A1 - Hanke, T. A1 - Todor, A. T1 - Ontopanel: a diagrams.net plugin for graphical semantic modelling N2 - Ontologies that represent a map of the concepts and relationships between them, are becoming an effective solution for data standardization and integration of different resources in the field of materials science, as efficient data storage and management is the building block of material digitization. However, building a domain ontology is not a simple task. It requires not only a collaborative effort between ontologists and domain experts, but also the modeling approaches and tools play a key role in the process. Among all approaches, graphical representation of domain ontologies based on standard conceptual modeling languages is widely used because of its intuitiveness and simplicity. Various tools have been developed to realize this approach in an intuitive way, such as Protégé plugins and web visualization tools. The Materials-open-Lab (MatOLab) project, which aims to develop ontologies and workflows in accordance with testing standards for the materials science and engineering domains, adopted a UML (Unified Modeling Language) approach based on the diagrams.net. It is a powerful, popular, open-source graphical editor. In practical case studies, however, many users’ needs could not be met, such as reusing ontology, conversion, and data mapping. Users must switch between different tools to achieve a certain step, and thereby invariably increase learning cost. The lack of validation also leads to incorrect diagrams and results for users who are not familiar with the ontology rules. To address these issues, we designed Ontopanel, a diagrams.net-based plugin that includes a set of pipeline tools for semantic modeling: importing and displaying protégé-like ontologies, converting diagrams to OWL, validating diagrams by OWL rules, and mapping data. It uses diagrams.net as the front-end for method modeling and Django as the back-end for data processing. As a web-based tool, it is very easy to expand its functionality to meet changing practical needs. T2 - MSE 2022 CY - Darmstadt, Germany DA - 27.09.2022 KW - Ontology KW - Tools KW - Material digital KW - Mat-o-lab KW - Graphic design KW - Ontology development KW - Data mapping KW - FAIR KW - Materials testing PY - 2022 AN - OPUS4-55884 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bayerlein, Bernd A1 - Zia, Ghezal-Ahmed A1 - Schilling, Markus A1 - Skrotzki, Birgit A1 - von Hartrott, P. A1 - Hanke, T. A1 - Waitelonis, J. T1 - Towards Interoperability: Digital Representation of a Material Specific Characterization Method N2 - Certain metallic materials gain better mechanical properties through controlled heat treatments. For example, in age-hardenable aluminum alloys, the strengthening mechanism is based on the controlled formation of nanometer sized precipitates, which represent obstacles to dislocation movement. Precise tuning of the material structure is critical for optimal mechanical behavior in the application. Therefore, analysis of the microstructure and especially the precipitates is essential to determine the ideal parameters for the interplay of material and heat treatment. Transmission electron microscopy (TEM) is utilized to identify precipitate types and orientations in a first step. Dark-field imaging (DF-TEM) is often used to image the precipitates and to quantify their relevant dimensions. The present work aims at the digital representation of this material-specific characterization method. Instead of a time-consuming, manual image analysis, an automatable, digital approach is demonstrated. Based on DF-TEM images of different precipitation states of a wrought aluminum alloy, a modularizable digital workflow for quantitative precipitation analysis is presented. The integration of this workflow into a data pipeline concept will also be discussed. Thus, by using ontologies, the raw image data, their respective contextual information, and the resulting output data from the quantitative precipitation analysis can be linked in a triplestore. Publishing the digital workflow and the ontologies will ensure the reproducibility of the data. In addition, the semantic structure enables data sharing and reuse for other applications and purposes, demonstrating interoperability. The presented work is part of two digitization initiatives, the Platform MaterialDigital (PMD, materialdigital.de) and Materials-open-Laboratory (Mat-o-Lab). T2 - MSE 2022 CY - Darmstadt, Germany DA - 27.09.2022 KW - Interoperability KW - Ontology KW - Precipitation Analysis PY - 2022 AN - OPUS4-55892 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Heuser, Lina A1 - Nofz, Marianne A1 - Müller, Ralf A1 - Deubener, J. T1 - Silver dissolution and precipitation in an Na2O–ZnO–B2O3 metallization paste glass N2 - Thermally stimulated interactions between silver and glass, that is, silver dissolution as Ag+ and precipitation as Ag0 were studied in two glass series of molar target composition xAg2O–(19 − x)Na2O–28ZnO–53B2O3 with x = 0, 0.1, 0.5, 5 and (19Na2O–28ZnO–53B2O3)+yAg2O with y = 0.01, 0.05. These act as model for low-melting borate glasses being part of metallization pastes. The occurrence of metallic silver precipitates in melt-quenched glass ingots demonstrated that silver dissolved only in traces (< 0.01 mol%) in the glasses. The dissolved silver was detected by means of Raman spectroscopy and energy-dispersive X-ray spectroscopy. Increasing x in the batch could not lead to a significant increase of the silver ion fraction in the glass as possible in binary silver borate glasses. In situ observation of heated AgNO3 mixed with the base glass frit in a hot stage microscope showed that Ag0 precipitation occurs already at the solid state. At higher temperatures, small droplets of liquid silver were found to move freely within the melt, whereas coalescence caused a stepwise increase of their size. These results contribute to the understanding of formation of silver precipitates in metallization pastes described in the literature. KW - Silver metallization paste KW - Batch reactions KW - Borate KW - Glass forming melts KW - Glass manufacturing KW - Raman spectroscopy PY - 2022 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-559433 DO - https://doi.org/10.1111/ijag.16613 SN - 2041-1286 SP - 1 EP - 11 PB - Wiley Online Library AN - OPUS4-55943 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Han, Ying A1 - Kruse, Julius A1 - Madia, Mauro A1 - Skrotzki, Birgit T1 - High cycle fatigue behavior of alloy EN AW-2618A N2 - The presentation shows the results of high cycle fatigue (HCF) tests from the aluminium alloy EN AW-2618A. This study investigates the mean stress influence in the T61 condition and the effect of overaging. For this purpose, axial HCF tests were carried out at room temperature and different stress ratios (R=-1, R=0.1) as well as with overaged conditions (T61+10h@230°C, T61+1000h@230°C). After completion of the tests, the fracture surfaces were examined to study crack initiation. T2 - The 18th International Conference on Aluminium Alloys CY - Toyama, Japan DA - 04.09.2022 KW - High Cycle Fatigue KW - Aluminium Alloy KW - EN AW-2618A PY - 2022 AN - OPUS4-55865 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Skrotzki, Birgit T1 - Aging processes in precipitation hardened aluminum alloys N2 - The mechanical strength of wrought high-strength aluminum alloys is essentially based on precipitation hardening, possibly in combination with prior forming, e. g. by stretching. Important parameters for achieving an optimum combination of hardness, strength, ductility, toughness, and further properties such as corrosion resistance are age-hardening temperature and time. During thermal (mechanical) treatment, nucleation and growth of precipitates takes place, leading to the desired degree of hardening. In aluminum alloys, precipitation sequences are usually passed through, i. e. a sequence of metastable precipitates is formed before the stable phase can precipitate. The optimum combination of properties is therefore based on a certain (optimum) microstructure, which can, however, change during the use of a component, since the microstructure is not stable. This happens in particular when the operating temperatures are close to the aging temperature and/or the operating times are sufficiently long. An external mechanical load may accelerate the processes. The presentation gives some examples for this. T2 - Materials Science and Engineering Congress MSE 2022 CY - Darmstadt, Germany DA - 27.9.2022 KW - Aluminium alloy KW - Precipitation hardening KW - Aging KW - Degradation PY - 2022 AN - OPUS4-55877 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Heuser, Lina A1 - Nofz, Marianne A1 - Müller, Ralf T1 - Alkali and alkaline earth zinc and lead borate glasses: Sintering and crystallization N2 - Glasses in the systems Me2O-ZnO-B2O3 with Me = Li, Na, K, Rb (MeZB), Na2O-ZnO-CuO-B2O3 (NZCuB), CaO-ZnO-B2O3 (CaZB), and Li2O-PbO-B2O3 (LPbB) as a reference, were studied by differential thermal analysis, dilatometry, rotational viscometry, and heating microscopy. A decrease of viscosity and sintering range was found with decreasing number of fourfold coordinated boron. The viscosity of the alkali zinc borate glasses varies only slightly. LPbB and CaZB stand out by their reduced and increased viscosities, respectively. Sodium, potassium, and calcium zinc borate glasses possess a fragility above 76. All glasses were sintered to full density before crystallization. Mostly binary zinc borate phases govern crystallization. A ternary crystalline phase was detected only in the potassium containing sample. The Weinberg glass stability parameter ranges between 0.07 and 0.12. This is caused by the presence of several crystalline phases and varying melting points of even the same crystalline phase in different glass matrices. KW - Alkali zinc borate glasses KW - Lead borate glasses KW - Viscosity KW - Sintering KW - Crystallization KW - Fragility PY - 2022 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-556128 DO - https://doi.org/10.1016/j.nocx.2022.100116 SN - 2590-1591 VL - 15 SP - 1 EP - 8 PB - Elsevier CY - Amsterdam AN - OPUS4-55612 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Diener, S. A1 - Schubert, Hendrik A1 - Held, A. A1 - Katsikis, N. A1 - Günster, Jens A1 - Zocca, Andrea T1 - Influence of the dispersant on the parts quality in slurry-based binder jetting of SiC ceramics N2 - Binder jetting is establishing more and more in the ceramic industry to produce large complex shaped parts. A parameter with a great impact on the quality of the parts is the binder–powder interaction. The use of ceramic slurries as feedstock for this process, such as in the layerwise slurry deposition–print technology, allows a great flexibility in the composition. Such slurries are typically composed of ceramic powder, water, and small amounts of various additives. The understanding of the effect of these components on the printing quality is thus essential for the feedstock development. Four models were developed regarding the impact of additives, such as dispersants on printing. These models were confirmed or rebutted by experiments performed for an SiC slurry system with two different concentrations of a dispersant and a commercial phenolic resin used as a binder. It is shown that for this system the influence of the dispersant on the curing behavior and the clogging of the pores by dispersant can be neglected. The redispersion of the dispersant after the curing of the resin has no or only a minor effect. However, the wetting behavior determined by the surface energies of the system seem to be most crucial. In case the surface energy of the slurry additive is significantly lower than the surface energy of the binder, the strength of the green parts and the printing quality will be low. This was shown by inverse gas chromatography, contact angle measurement, rheological characterization, and mechanical tests with casted samples. KW - Additive Manufacturing KW - Binder Jetting KW - Layerwise slurry deposition KW - Silicon carbide KW - Wetting PY - 2022 DO - https://doi.org/10.1111/jace.18693 SN - 1551-2916 VL - 2022 SP - 1 EP - 15 PB - Wiley-Blackwell CY - Oxford AN - OPUS4-55542 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Zocca, Andrea A1 - Schubert, Hendrik A1 - Günster, Jens T1 - Additive Manufacturing of advanced ceramics by layerwise slurry deposition and binder jetting (LSD-print) N2 - Powder bed technologies are amongst the most successful Additive Manufacturing (AM) techniques. Powder bed fusion and binder jetting especially are leading AM technologies for metals and polymers, thanks to their high productivity and scalability. The application of these techniques to most ceramics has been difficult so far, because of the challenges related to the deposition of homogeneous powder layers when using fine powders. In this context, the "layerwise slurry deposition" (LSD) has been developed as a layer deposition method which enables the use of powder bed AM technologies also for advanced ceramic materials. The layerwise slurry deposition consists of the layer-by-layer deposition of a ceramic slurry by means of a doctor blade, in which the slurry is deposited and dried to achieve a highly packed powder layer. This offers high flexibility in the ceramic feedstock used, especially concerning material and particle size. The LSD technology can be combined with binder jetting to develop the so-called “LSDprint” process for the additive manufacturing of ceramics. The LSDprint technology combines the high-speed printing of binder jetting with the possibility of producing a variety of high-quality ceramics with properties comparable to those achieved by traditional processing. In this presentation, the LSD process will be introduced and several examples of application ranging from silicate to high-performance ceramics will be shown. Recent developments towards the scale-up and industrialization of this process will be discussed, alongside future perspectives for the multi-material additive manufacturing. T2 - Ceramics in Europe 2022 CY - Krakow, Poland DA - 10.07.2022 KW - Layerwise slurry deposition KW - Laser induced slipcasting KW - Additive Manufacturing KW - Ceramics PY - 2022 AN - OPUS4-55543 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Heuser, Lina A1 - Nofz, Marianne T1 - Alkali and alkaline earth zinc and lead borate glasses: Structure and properties N2 - Low melting Li2O-PbO-B2O3, Me2O-ZnO-B2O3, Me = Li, Na, K, Rb and CaO-ZnO-B2O3 glasses were studied with Raman and infrared spectroscopies to advance the structural understanding of zinc borate glasses as potential candidates for substitution of lead containing glasses. Although the effect of type of alkali ions on the number (N4) of fourfold coordinated boron (B4) in the glasses is small, the alkali ions direct the type of borate groups, i.e., pentaborate in lithium, sodium, and calcium zinc borate glasses, as well as diborate in potassium and rubidium containing ones. Both groups were simultaneously found in Li2O-PbO-B2O3. Alkali ions are mainly responsible for the formation of B4-units and metaborate. Zinc ions favorably compensate non-bridging oxygen and partially form ZnO4. With decreasing N4 and field strength of the alkali ions the atomic packing density, glass transition temper ature and Young’s Modulus also decrease. The coefficient of thermal expansion increases with decreasing N4. KW - Raman spectroscopy KW - IR spectroscopy KW - Alkali zinc borate glasses KW - Lead borate glasses KW - Physical properties KW - Young’s Modulus PY - 2022 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-556109 DO - https://doi.org/10.1016/j.nocx.2022.100109 SN - 2590-1591 VL - 15 SP - 1 EP - 12 PB - Elsevier CY - Amsterdam AN - OPUS4-55610 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Abel, Andreas A1 - Zapala, P. A1 - Michels, H. A1 - Skrotzki, Birgit T1 - Ambient and high-temperature mechanical properties of intermetallic Fe3Al alloys with complex borides N2 - Due to the increasing scarcity of critical raw materials current high-temperature materials are sought to be replaced by alloys based on more abundant metals. One possibility within the class of intermetallics are iron aluminides, which combine sustainability and cost-efficiency with the prospect of mass savings. Iron aluminides show competitive specific strength up to 700 °C and excellent creep and wet corrosion resistance by small additions of Mo, Ti and B. Nevertheless, a Mo content of above 2 at.% which is needed for optimum corrosion resistance results in enhanced brittleness, especially at room temperature. This is why alloys with these Mo fractions were only mechanically tested under compressive loading so far. Still, testing of static and creep properties under tensile loading is required for reliable component design. Besides high standards for crack-free processing, data acquisition for tensile loads is especially complicated by environmental embrittling effects for iron aluminides. To cope with these challenges, the AiF research project “WAFEAL – Materials applications for iron aluminides” was initiated. The main goal is to collect standardised data on ambient and high-temperature tensile properties and creep properties. Samples with a nominal composition of Fe-26Al-4Mo-0.5Ti-1B [at.%] were manufactured via centrifugal casting in ceramic shell moulds followed by machining. Heat treatment for homogenisation and final polishing were carried out where appropriate. A summary of the achieved tensile and creep properties such as yield and tensile strength, maximum elongation, secondary creep rate and stress exponents will be given. Results will be also discussed regarding the influence of temperature, stress level and microstructure on the damage mechanisms. Furthermore, the effect of different alloy concentrations on the mechanical response at different temperatures will be outlined within a small experimental series. T2 - MSE Congress 2022 CY - Darmstadt, Germany DA - 27.09.2022 KW - Fe-Al alloys KW - Intermetallics KW - Iron aluminides KW - Tensile data KW - High temperature mechanical properties KW - Creep data KW - Fractography PY - 2022 AN - OPUS4-55993 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Maximilian, Thuy A1 - Spyrantis, Alexander A1 - Böhning, Martin A1 - Niebergall, Ute A1 - Maaß, Robert T1 - Spatially resolved roughness exponent in polymer fracture N2 - The fracture surface of slow and continuous crack propagation during environmental stress cracking of a semicrystalline polyethylene exhibits isotropic roughness exponents at the local scale but resolved across the macroscopic fracture surface a clear position dependence is found. The spatially resolved roughness exponent admits values in the range between 0.1 and 0.4, demonstrating nontrivial exponents in the small length-scale regime. Instead, they vary across the fracture surface according to the stress-state distribution, which suggests that the exponents are intimately linked to the locally dominating dissipation processes during craze cracking. KW - Plasticity KW - Fracture KW - Material failure KW - Mechanical deformation PY - 2022 DO - https://doi.org/10.1103/PhysRevMaterials.6.L090601 VL - 6 IS - 9 SP - 1 EP - 7 PB - American Physical Society CY - USA, Maryland AN - OPUS4-55797 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Rizzardi, Q. A1 - Derlet, P. M. A1 - Maaß, Robert T1 - Intermittent microplasticity in the presence of a complex microstructure N2 - We demonstrate the gradual shift from scale-free intermittent microplasticity to a scale-dependent behavior via the introduction of a variety of microstructural features within the Al-Cu binary alloy system. As long as the obstacles to dislocation motion remain shearable, the statistics of intermittent microplasticity has fat-tailed contributions. The introduction of incoherent precipitates leads to a complete transition from scale-free powerlaw scaling to an exponential and scale-dependent distribution. These results demonstrate how non-Gaussian interactions survive across different microstructures and further suggest that characteristic microstructural length scales and obstacle pinning-strengths are of secondary importance for the intermittency statistics, as long as dislocations can shear their local environment. KW - Scale-dependent behavior KW - Al-Cu binary alloy system PY - 2022 DO - https://doi.org/10.1103/PhysRevMaterials.6.073602 SN - 2475-9953 VL - 6 IS - 7 SP - 1 EP - 9 PB - American Physical Society AN - OPUS4-55387 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Maaß, Robert T1 - The Federal Institute of Materials Research and Testing (BAM) – 150 Years of Enabling Scientific and Technological Breakthrough N2 - BAM! This issue of Advanced Engineering Materials celebrates 150 years of scientific and technical research at the interface between academia, industry and politics. Rooted in 1871 at the birth of the German Empire and at that time located in simple basements and barracks, the institutional development began around mechanical metallurgy of iron and steel and represents today a diverse portfolio of fore-front research that orients itself along tomorrow's societal challenges and long-term research horizons. KW - 150 Years KW - Adolf Martens PY - 2022 DO - https://doi.org/10.1002/adem.202200648 VL - 24 IS - 6 SP - 1 EP - 3 PB - Wiley-VCH GmbH AN - OPUS4-55388 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Ghafafian, Carineh A1 - Trappe, Volker T1 - Fully-reversed fatigue behavior of scarf joint repairs for wind turbine blade shell applications N2 - Due to manufacturing imperfections which can propagate to damage under in-service loads, wind turbine rotor blades, made primarily of glass fiber reinforced polymers (GFRP), often fail significantly before their design life. To enable a quick and cost-effective return to service, localized repairs can be executed by technicians in the field, directly accessing the blades by suspended roping. Scarf joint repairs, shown to be highly efficient with a smooth load transition across angled joint walls and a restored aerodynamic profile, are the focus of this study. The damage mechanisms of these structures were examined under fully-reversed mechanical cyclic loading with a load ratio R = -1, which was made possible on the coupon scale by a custom designed anti-buckling support. The number of cycles to failure were compared across load levels. While the scarf joint ratio was held constant at 1:50, known from industry and literature to be a good compromise between restored mechanical properties and repair size, the layup sequence was varied between small-to-large and large-to-small. Hereby the effect of the presence of resin pockets and fiber orientation mismatch between the parent and repair structure on the failure mechanism as well as fatigue strength of ±45° GFRP scarf joint repair structures was studied. Strain development across the joint length was measured to assess stiffness degradation in addition to the fatigue strength recovery of scarf joint structures with respect to pristine reference specimens. Grayscale analysis was used to monitor the damage state leading to fracture across the specimens. Post-mortem fractography analysis with light microscopy described the global failure mechanisms as well as local damage distribution within the structure, all of which provided insight to critical variables in scarf joint GFRP structures under fully-reversed mechanical cyclic loading, allowing for the tailoring of such repairs on wind turbine blade shells for maximum restoration of service life. T2 - 20th European Conference on Composite Materials (ECCM20) CY - Lausanne, Switzerland DA - 26.06.2022 KW - Glass fiber reinforced polymers KW - Scarf repairs KW - Fatigue PY - 2022 AN - OPUS4-55638 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Cestari, F. A1 - Yang, Y. A1 - Wilbig, Janka A1 - Günster, Jens A1 - Motta, A. A1 - Sglavo, V. T1 - Powder 3D printing of bone scaffolds with uniform and gradient pore sizes using cuttlebone-derived calcium phosphate and glass-ceramic N2 - The pore geometry of bone scaffolds has a major impact on their cellular response; for this reason, 3D printing is an attractive technology for bone tissue engineering, as it allows for the full control and design of the porosity. Calcium phosphate materials synthesized from natural sources have recently attracted a certain interest because of their similarity to natural bone, and they were found to show better bioactivity than synthetic compounds. Nevertheless, these materials are very challenging to be processed by 3D printing due to technological issues related to their nanometric size. In this work, bone scaffolds with different pore geometries, with a uniform size or with a size gradient, were fabricated by binder jetting 3D printing using a biphasic calcium phosphate (BCP) nanopowder derived from cuttlebones. To do so, the nanopowder was mixed with a glass-ceramic powder with a larger particle size (45–100 µm) in 1:10 weight proportions. Pure AP40mod scaffolds were also printed. The sintered scaffolds were shown to be composed mainly by hydroxyapatite (HA) and wollastonite, with the amount of HA being larger when the nanopowder was added because BCP transforms into HA during sintering at 1150 ◦C. The addition of bio-derived powder increases the porosity from 60% to 70%, with this indicating that the nanoparticles slow down the glass-ceramic densification. Human mesenchymal stem cells were seeded on the scaffolds to test the bioactivity in vitro. The cells’ number and metabolic activity were analyzed after 3, 5 and 10 days of culturing. The cellular behavior was found to be very similar for samples with different pore geometries and compositions. However, while the cell number was constantly increasing, the metabolic activity on the scaffolds with gradient pores and cuttlebone-derived powder decreased over time, which might be a sign of cell differentiation. Generally, all scaffolds promoted fast cell adhesion and proliferation, which were found to penetrate and colonize the 3D porous structure. KW - Bioactivity KW - Cuttlefish KW - Biphasic calcium phosphate KW - Binder jetting KW - Scaffold geometry KW - Hausner ratio PY - 2022 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-553627 DO - https://doi.org/10.3390/ma15155139 SN - 1996-1944 VL - 15 IS - 15 SP - 1 EP - 16 PB - MDPI CY - Basel AN - OPUS4-55362 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Thuy, Maximilian A1 - Niebergall, Ute A1 - Oehler, H. A1 - Alig, I. A1 - Böhning, Martin T1 - Damaging effect of admixtures used in crop protection products on high density polyethylene packaging material N2 - The phenomenon of environmental stress cracking is still a major issue in materials engineering as well as from a scientific perspective. Especially in the case of packaging materials made of high-density polyethylene, assessing the potential of premature damage due to environmental stress cracking is complex because of the large number of components in possible liquid filling goods. As a first guideline, the well-known effect of detergents and dispersants is usually considered, but the interplay with other components, such as organic solvents is often unknown. Particularly challenging in this respect are crop protection products, consisting of several different admixtures in addition to the biologically active ingredients. This study is based on two model liquids representing these admixtures that were established for testing in this context. The model liquids as well as their constituting components were used as liquid media in the Full Notch Creep Test to characterize the environmental stress cracking behavior of a typical high-density polyethylene. Complementary to the time-to failure of a notched specimen obtained from these tests, the crack opening was monitored optically, and the fracture surface was analyzed post-failure by laser scanning microscopy as well as scanning electron microscopy. Based on the results, the effect of various surfactants as well as the influence of organic solvents on environmental stress cracking are discussed. KW - Environmental stress cracking KW - High-density polyethylene KW - Crop protection products KW - Full notch creep test KW - Fracture surface analysis KW - Crack opening displacement PY - 2022 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-554631 DO - https://doi.org/10.1016/j.polymertesting.2022.107672 SN - 0142-9418 VL - 114 SP - 1 EP - 16 PB - Elsevier Ltd. CY - Amsterdam AN - OPUS4-55463 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Schönauer-Kamin, Daniela A1 - Hetzel, K. A1 - Moos, R. A1 - Bresch, Sophie T1 - Powder-Aerosol deposited (PAD) calcium manganate as n-type thermoelectric material N2 - Currently, calcium manganate CaMnO3 and calcium cobaltite Ca3Co4O9 are being investigated as n-type resp. p-type semiconducting materials as oxidation- and temperature-resistant thermoelectric materials for oxide multilayer thermoelectric generators (TEGs). In order to manufacture multilayer TEGs, pressure-assisted sintering processes at high temperatures are necessary to achieve optimal thermoelectric material properties. To realize TEGs in planar film technology, another method to obtain dense ceramic layers directly from the synthesized starting powders without a subsequent high temperature step is emerging recently: the powder aerosol deposition (PAD) method. In the present work, it is investigated whether PAD is suitable to produce dense ceramic films from Sm-doped CaMnO3 and Ca3Co4O9 powders. The resulting thermoelectric properties are characterized as a function of temperature. CaMnO3 powder could successfully be processed by PAD with resulting layer thicknesses of 5- 6 µm without any high-temperature sintering steps of the films. The electrical conductivity and the Seebeck coefficient of the films were determined in-plane from room temperature to 600 °C in air. The results show a Seebeck coefficient of around -200 µV/K, which is comparable to results of pressed and sintered bars. At 400 °C, the electrical conductivity corresponds to the conductivity of the bar. At higher temperatures the conductivity is better than with the reference. Below 400°C, the electrical conductivity is somewhat lower than that of the reference sample, a mild thermal treatment of the PAD layer improves it. It is expected that the thermal conductivity of the PAD film will be lower compared to the bars due to the nano-crystalline film morphology. This should result in a significantly increased ZT value for the PAD layers and a higher efficiency of the TEG. The work shows that both CaMnO3 and Ca3Co4O9 can be successfully processed by PAD, and the PAD films show comparable thermoelectric properties. T2 - 18th European Conference on Thermoelectrics CY - Barcelona, Spanien DA - 14.09.2022 KW - Film depositition KW - Calcium cobaltite PY - 2022 AN - OPUS4-55771 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN ED - Hennecke, M. ED - Skrotzki, Birgit T1 - Hütte Band 2: Grundlagen des Maschinenbaus und ergänzende Fächer für Ingenieure N2 - Die HÜTTE ist ein Kompendium und Nachschlagewerk für unterschiedliche Aufgabenstellungen. Durch Kombination der Einzeldisziplinen dieses Wissenskreises kann das multidisziplinäre Grundwissen für die verschiedenen Technikbereiche und Ingenieuraufgaben zusammengestellt werden. Die HÜTTE enthält in drei Bänden - orientiert am Stand von Wissenschaft und Technik und den Lehrplänen der Technischen Universitäten und Hochschulen - die Grundlagen des Ingenieurwissens. Band 2 enthält die Grundlagen des Maschinenbaus und ergänzende Fächer. KW - Grundlagen des Maschinenbaus PY - 2022 SN - 978-3-662-64371-6 DO - https://doi.org/10.1007/978-3-662-64372-3 SN - 2522-8188 SP - 1 EP - 967 PB - Springer Vieweg CY - Berlin ET - 35 AN - OPUS4-55740 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Heuser, Lina A1 - Müller, Ralf A1 - Nofz, Marianne A1 - Deubener, J. T1 - Liquid phase sintering of alkali zinc borate glass-bearing silver pastes for applications in photovoltaics and microelectronics N2 - Liquid phase sintering of glass bearing silver pastes used in photovoltaics and microelectronics is poorly understood. In particular, the role of different network modifiers acting in the glass component and the question of the most suitable atmospheric oxygen level during sintering are still under considerable debate. To tackle these issues, low-melting and lead-free X2O-ZnO-B2O3 glasses with X = Li, Na, K and Rb (LZB, NZB, KZB and RZB) were prepared. Infrared spectroscopy showed that the glass structure was similar to each other, while an increase of tetrahedrally coordinated boron with increasing field strength of the alkali was evident. In turn, the glass transition temperature (from differential thermal analysis) increased in the order: RZB (449 °C) < KZB (460 °C) < NZB (465 °C) < LZB (472 °C). Powders of each glass were mixed with organics to receive silver-glass-pastes containing 30 vol% glass and these were subjected to heating microscopy in air. Although similar onset temperatures of sintering were recorded for Ag-NZB and Ag-LZB glass pastes, and for Ag-RZB paste and KZB-Ag-paste, respectively, differences in the crystallization behavior and final densification were observed between the former and the latter group. These were translated in terms of differences in silver dissolution and reprecipitation among the two groups. Further, running the experiments in nitrogen gas showed that sintering of all pastes was considerably hampered. The slow-down of the sinter kinetics was found to be in line with the assumed lower oxidation and dissolution of silver ions into the glass-forming liquid. T2 - 26th International Congress on Glass CY - Berlin, Germany DA - 03.07.2022 KW - Silver metallization paste KW - Sintering KW - Glass KW - Alkali zinc borate glasses KW - Viscosity KW - Structure PY - 2022 AN - OPUS4-55728 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Heuser, Lina A1 - Roßmöller-Felz, Mattis A1 - Nofz, Marianne A1 - Müller, Ralf A1 - Deubener, J. T1 - In situ observation of silver precipitation in sodium zinc borate glass-forming melts N2 - Melting of Na2CO3-ZnO-B2O3 batches containing up to 16.8 wt% AgNO3 (5 mol% Ag2O in the target glass composition) was observed in situ by means of hot stage microscopy. In all batches metallic silver precipitation took place as most of the silver nitrate was reduced to metallic silver before Ag+ ions could be dissolved in the evolving borate melts. In turn, only traces of Ag+ (<300 ppmw) were dissolved in the sodium zinc borate glass melts under study. It is assumed that the oxidation to Ag+ was limited due to poor availability of reducible oxygen in the glass melts and presence of Na2O being a stronger base than Ag2O. Thus, the precipitated metallic silver formed droplets of different sizes. The larger droplets (d > 20 µm) were already settled at the bottom of the container and remained constant in size upon dwelling for 1 h at 1050 °C of about one hour and the subsequent cooling (45 K/min) to room temperature, whereas the smaller droplets (d < 20 µm) were mobile in the borate melt due to Marangoni and Stokes motion. For the latter droplets, coalescence was observed in situ. A growth of larger droplets at the expense of smaller ones, i.e., Ostwald ripening was also expected but could not be studied with the used experimental equipment. T2 - 26th International Congress on Glass CY - Berlin, Germany DA - 03.07.2022 KW - Glass melt KW - Silver KW - Sodium zinc borate glass KW - Hot stage microscopy KW - Precipitation PY - 2022 AN - OPUS4-55732 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Heuser, Lina A1 - Nofz, Marianne A1 - Sobek, Pascal A1 - Körner, Stefan A1 - Eberstein, Markus A1 - Müller, Ralf T1 - Flüssigphasensinterung von Silber-Glas Dispersionen N2 - Silber-Glas Wechselwirkungen spielen eine wichtige Rolle zum Beispiel in Glas-haltigen Silberpasten, die in der Photovoltaik oder Mikroelektronik verwendet werden. Um ein besseres Verständnis der Vorgänge zu erhalten, werden niedrig-schmelzende, bleifreie X2O ZnO B2O3 Gläser (X = Li, Na, K und Rb, Abk.: LZB, NZB, KZB and RZB) zur Untersuchung der Pasten verwendet. Raman und Infrarot Spektroskopie zeigen, dass die Glasstruktur weitgehend vergleichbar ist, aber Unterschiede in der Bildung von Pentaboratgruppen in LZB und NZB oder Diboratgruppen in KZB und RZB auftreten. Die Anzahl an vierfach koordinierten Bor-Ionen (N4) sinkt mit zunehmendem Alkaliionenradius. Die Verringerung von N4 führt zu einer niedrigeren Glasübergangstemperatur in der Reihe LZB (472 °C) < NZB (465 °C) < KZB (460 °C) < RZB (449 °C). Zur Herstellung der Pasten wurde kommerzielles Silber-Pulver mit 30 Vol.-% Glas und Organik gemischt. Das Sinterverhalten der gepressten Pulver wurde mittels Erhitzungsmikrospie untersucht. Der Sinterbeginn der Pasten ist vergleichbar und korrespondiert mit den geringen Unterschieden der Viskosität bei vergleichbarer Partikelgröße der Gläser. In den Ag-KZB- und Ag-RZB-Pasten ist die Schwindung durch die stärker einsetzende Kristallisation im Vergleich zu LZB und NZB verzögert. T2 - AK Glasig-kristalline Multifunktionswerkstoffe CY - Aachen, Germany DA - 17.02.2022 KW - Sintern KW - Silber KW - Glas KW - Diffusion KW - Gefüge PY - 2022 AN - OPUS4-55735 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Junge, P. A1 - Stargardt, Patrick A1 - Kober, D. A1 - Greinacher, M. A1 - Rupprecht, C. T1 - Thermally Sprayed Al2O3 Ceramic Coatings for Electrical Insulation Applications N2 - Thermal spraying enables a fast and propelling way to additively deposit various ceramics as electric insulators, which are used in conditions where polymers are not suitable. Alumina (Al2O3) is among the most employed materials in the coating industry since it exhibits good dielectric properties, high hardness, high melting point while still being cost-effective. Various parameters (e.g. feedstock type, plasma gas mixture, plasma power) significantly influence the resulting coating in terms of microstructure, porosity, crystallinity, and degree of un-or molten particles. As a consequence, these parameters need to be investigated to estimate the impact on the electrical insulating properties of thermally sprayed alumina. This study focuses on the development of a novel electric insulation coating from Al2O3 feedstock powders deposited via atmospheric plasma spray (APS). The microstructure, porosity, and corresponding crystallographic phases have been analyzed with optical microscopy, XRD, and SEM images. To achieve an understanding of the parameters influencing the electrical insulation performance of the manufactured coatings, an in-depth analysis of the fundamental dielectric parameters e.g., DC resistance, breakdown strength, dielectric loss tangent, permittivity is presented. T2 - International Thermal Spray Conference and Exposition 2022 CY - Vienna, Austria DA - 04.05.2022 KW - Thermal Spray KW - Alumina KW - Dielectric properties PY - 2022 SP - 1 EP - 8 AN - OPUS4-55821 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER -