TY - JOUR A1 - Blaeß, Carsten A1 - Müller, Ralf T1 - Viscous crack healing in soda–lime–magnesium–silicate–ZrO2 glass matrix composites N2 - AbstractThe present study investigates the influence of the crystal volume content on viscous crack healing in glass ceramic glass sealants. To ensure constant microstructure during healing, soda–lime–magnesium silicate glass matrix composites with varied volume fractions of ZrO2 filler particles were used. Crack healing was studied on radial cracks induced by Vickers indentation, which were stepwise annealed to monitor the healing progress by confocal laser scanning microscopy. Confirming previous studies, healing of radial cracks in pure glass was found delayed by global flow phenomena like crack widening and crack edge and tip rounding to minimize the sample surface. With increasing ZrO2 filler content, these global flow phenomena were progressively inhibited whereas local flow phenomena like sharp crack tip healing could still occur. As a result, crack healing was even accelerated by filler particles up to a maximum filler content of 17 vol% whereas crack healing was fully suppressed only at 33 vol% filler content. KW - Crack healing KW - Glass matrix composite KW - Solid oxide fuell cell KW - Vickers identation KW - Viscosity PY - 2024 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-607860 DO - https://doi.org/10.1111/jace.20002 SN - 0002-7820 SP - 1 EP - 12 PB - Wiley AN - OPUS4-60786 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Blaeß, Carsten A1 - Müller, Ralf T1 - Fast crack healing in glass-matrix composites with rigid filler percolation frameworks N2 - To ensure the durability of solid oxide fuel cell sealants, the understanding of the microstructural influence on viscous crack healing is essential. To this end, the effect of microstructure with respect to the spatial distribution of filler particles on viscous crack healing was studied with confocal laser scanning microscopy in glass-matrix composites (GMCs) made by mix-milling and sintering of sodalime magnesium silicate glass and Φ ≈ 6 vol% ZrO2 chemically inert rigid filler particles. This way, no change in Φ occurred during the crack healing treatments studied on Vickers indentation-induced radial cracks in polished GMC surfaces. Different microstructures were mimicked using different ZrO2 particle sizes for mix-milling. Unlike coarse ZrO2 particles, similar in size to the glass particle, fine ZrO2 particles, much smaller than the glass particles, form a rigid percolation framework (RPF) of ZrO2 filler particles around the former glass particles or glass particle agglomerates. For this RPF microstructure, crack healing was observed more readily as crack healing retardation phenomena like large-scale crack widening and crack tip rounding were strongly reduced, whereas narrow cracks could still heal locally within the glassy regions. KW - Crack healing KW - Glass matrix composite KW - Rigid percolation frameworks KW - Vickers indentation PY - 2025 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-625921 DO - https://doi.org/10.1111/jace.20386 SN - 0002-7820 SP - 1 EP - 10 PB - Wiley AN - OPUS4-62592 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER -