TY - JOUR A1 - Zerbst, Uwe T1 - Application of fracture mechanics to welds with crack origin at the weld toe—a review. Part 2: welding residual stresses. Residual and total life assessment N2 - The two-part paper series provides an overview on the state-of-the-art in the application of engineering fracture mechanics to weldments limited to butt and fillet welds with crack initiation at weld toes. In the present second part, one focus is on welding residual stresses, their characteristics and stability under cyclic loading and their effect on structural integrity. Subsequently, features will be addressed which are essential for applying fracture mechanics to overall fatigue life and fatigue strength considerations of weldments. These comprise fatigue life relevant initial crack sizes and multiple crack initiation and Propagation due to various stress peaks along the weld toe. A concept is briefly introduced which covers all these aspects. KW - Fracture mechanics KW - Welding residual stresses KW - Multiple crack propagation KW - Fatigue strength PY - 2020 DO - https://doi.org/10.1007/s40194-019-00816-y VL - 64 IS - 1 SP - 151 EP - 169 PB - Springer AN - OPUS4-50263 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Werner, Tiago A1 - Madia, Mauro A1 - Zerbst, Uwe T1 - Comparison of the fatigue behavior of wrought and additively manufactured AISI 316L N2 - Additive manufacturing (AM) is becoming increasingly important in engineering applications due to the possibility of producing components with a high geometrical complexity allowing for optimized forms with respect to the in-service functionality. Despite the promising potential, AM components are still far from being used in safety-relevant applications, mainly due to a lack of understanding of the feedstock-process-properties-performance relationship. This work aims at providing a full characterization of the fatigue behavior of the additively manufactured AISI 316L austenitic stainless steel and a direct comparison with the fatigue performance of the wrought steel. To this purpose, a set of specimens has been produced by laser powder bed fusion (L-PBF) and subsequently heat treated at 900 °C for 1 hour for complete stress relief, whereas a second set of specimens has been machined out of hot-rolled plates. Low cycle fatigue (LCF) and high cycle fatigue (HCF) tests have been conducted for characterizing the fatigue behavior. The L-PBF material had a higher fatigue limit and better finite life performance compared to wrought material. Both, LCF and HCF-testing revealed an extensive cyclic softening. T2 - FATIGUE DESIGN 2021 CY - Online meeting DA - 17.11.2021 KW - Additive manufacturing KW - L-PBF KW - 316L KW - Fatigue KW - LCF KW - HCF PY - 2022 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-544952 DO - https://doi.org/10.1016/j.prostr.2022.03.056 SN - 2452-3216 VL - 38 SP - 554 EP - 563 PB - Elsevier B.V. AN - OPUS4-54495 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Zhu, Jiangchao A1 - Schurig, M. A1 - Schlums, H. A1 - Madia, Mauro A1 - Zerbst, Uwe T1 - Bruchmechanische Bewertung der Integrität einer Turbinenscheibe bei Überdrehzahl N2 - Turbinenscheiben sind thermisch und mechanisch hochbeanspruchte, sicherheitsrelevante Komponenten in Gasturbinen. Ihre Integrität wird in Bauteiltests unter Überdrehzahlbedingungen nachgewiesen. Kontext des Aufsatzes ist die Erarbeitung einer zusätzlichen Bewertungsebene auf der Grundlage von Versuchen unter monotoner Beanspruchung, die die Beanspruchung im Bauteil realistisch wiedergeben soll. Betrachtet wird ein halbelliptischer Riss, der bei der weiteren Ausbreitung als Umfangsriss wächst (rim peeling). Die Simulation dieser Stelle im Bauteil schließt die mechanische und thermische Beanspruchung sowie sie Dehnungsbehinderung ein. Letztere wird anhand zweier Parameter, der Spannungsmehrachsigkeit ℎ und des (allerdings modifizierten) Constraint-Parameters nach Newman, der die Spannungen über den plastisch verformten Bereich mittelt, bestimmt. Erwartungsgemäß zeigt sich, dass die höchste Dehnungsbehinderung weder an den Oberflächenpunkten, noch an den tiefsten Punkten, sondern an einer Stelle zwischen beiden auf der Rissfront auftritt. Als Versuchsgeometrie für die monotonen Tests soll eine Kreuzprobe mit wanddurchdringenden Rissen ausgehend von einer Innenbohrung dienen. Durch geeignete Wahl der Risstiefe sowie der in beiden Richtungen angreifenden Kräfte gelingt es, bauteiladäquate Zustände zu erzeugen. T2 - 54. Tagung des DVM-Arbeitskreises Bruchmechanik und Bauteilsicherheit CY - Online meeting DA - 22.02.2022 KW - Bruchmechanik KW - Struktur Integrität KW - Turbinenscheibe KW - Constraint PY - 2022 SP - 13 EP - 22 AN - OPUS4-54403 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Zhu, Jiangchao A1 - Madia, Mauro A1 - Schurig, M. A1 - Schlums, H. A1 - Zerbst, Uwe T1 - Fracture mechanics-based structural integrity assessment of aeroengine turbine disks under overspeed conditions N2 - Aero-engine turbine disks are safety-relevant components which are operated under high thermal and mechanical stress conditions. The actual part qualification and certification procedures make use of spin-tests conducted on productionsimilar disks. While these tests provide, on the one hand, a reliable definition of the critical conditions for real components, on the other hand they represent a relevant cost item for engine manufacturers. The aim of this work is to present part of a fracture mechanics-based procedure under development which aims at replacing the tests on production-similar disks with lab tests on fracture mechanics specimens. In particular, the rimpeeling failure mode is considered as case study. A semi-circular surface crack is modelled at the most stressed region at the diaphragm of a turbine disk, with the crack plane perpendicular to the radial direction. The crack is therefore subjected to a biaxial stress state and grows under increasing rotational speed until it triggers the rim-peeling failure. The finite element simulation of the cracked disk considers the real thermal and mechanical loading conditions. In order to design a lab representative specimen, beside the crack driving force, expressed in terms of � -integral, also the constraint to plastic deformation e.g., stress triaxiality, at the crack-tip must be similar for the same crack in the specimen and in the disk. This has been achieved and as expected, both the highest � -integral and constraint factor are calculated at the same location along the crack front for both disk and specimen. The results of the structural integrity assessment in the form of a Failure Assessment Diagram (FAD) show good agreement between designed specimen and disk both in terms of expected failure mode and value of the critical speed. Probabilistic aspects are also considered in the calculations. T2 - ASME Turbo Expo 2022: Turbomachinery Technical Conference and Exposition (GT2022) CY - Rotterdam, The Netherlands DA - 13.06.2022 KW - Fracture mechanics KW - Burst KW - Turbine disk PY - 2022 SP - 1 EP - 7 PB - ASME AN - OPUS4-55903 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Scacco, F. A1 - Zerbst, Uwe A1 - Meneghetti, G. A1 - Madia, Mauro T1 - Comparison between PSM and IBESS approaches for the fatigue life estimation of weldments N2 - In the framework of the fatigue assessment of welded components, several methods are available in design standards such as the nominal stress, hot-spot stress, notch stress and linear elastic fracture mechanics approaches. The present paper aims at comparing two advanced local approaches for the fatigue strength assessment of different welded joints made of steel. The first one is IBESS which is based on short crack fracture mechanics. The second one is the PSM which instead involves the strain energy density approach. Both methods will be briefly presented, and the fatigue life prediction results discussed. The results obtained for the joint geometries considered in this work show advantages and drawbacks of the approaches, which are thoroughly analysed as well. KW - Fatigue KW - Welded joints KW - FAT class KW - IBESS KW - Peak stress method (PSM) KW - Finite element (FE) PY - 2022 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-545139 DO - https://doi.org/10.1007/s40194-022-01284-7 SP - 1 EP - 23 PB - Springer AN - OPUS4-54513 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Madia, Mauro A1 - Zerbst, Uwe A1 - Werner, Tiago T1 - Estimation of the Kitagawa-Takahashi diagram by cyclic R curve analysis N2 - The Kitagawa-Takahashi (KT) diagram is a proven concept for describing the fatigue limit in presence of a defect or crack. It can be determined empirically with great experimental effort. It can also be estimated by means of the El Haddad relationship if the endurance limit and the long fatigue crack propagation threshold are available in reasonable accuracy. A third option is the determination using the cyclic R-curve, which describes the dependency of the fatigue crack propagation threshold on the crack growth at the short crack propagation stage. This can be experimentally determined using a closure-free initial pre-crack. It can then be applied to the determination of crack arrest for a given applied load and a given defect or crack size. Compared to the other two methods mentioned above, this option has considerable advantages: It can be applied to any component and any stress ratio. It allows the treatment of multiple cracks and provides estimations of the S-N curve in the finite life regime as well as at the endurance limit. Compared to the empirical determination of the KT diagram, the experimental effort is significantly lower and compared to the El Haddad approach it avoids problems such as the use of non-conservative long fatigue crack propagation thresholds (when the conventional load reduction method is applied to materials prone to corrosion) and the mathematical predetermination of the curve shape. The work introduces the method and provides a critical discussion as well as quantitative comparison between the different methods. T2 - FATIGUE DESIGN 2021 CY - Online meeting DA - 17.11.2021 KW - Fatigue life KW - Endurance limit KW - Kitagawa-Takahashi diagram KW - Cyclic R-curve PY - 2022 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-544931 DO - https://doi.org/10.1016/j.prostr.2022.03.032 SN - 2452-3216 VL - 38 SP - 309 EP - 316 PB - Elsevier B.V. AN - OPUS4-54493 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Schönherr, J. A. A1 - Duarte, Larissa A1 - Madia, Mauro A1 - Zerbst, Uwe A1 - Geilen, M. B. A1 - Klein, M. A1 - Oechsner, M. T1 - Robust determination of fatigue crack propagation thresholds from crack growth data N2 - The robust determination of the threshold against fatigue crack propagation DKth is of paramount importance in fracture mechanics based fatigue assessment procedures. The standards ASTM E647 and ISO 12108 introduce operational definitions of DKth based on the crack propagation rate da/dN and suggest linear fits of logarithmic DK– da/dN test data to calculate DKth. Since these fits typically suffer from a poor representation of the actual curvature of the crack propagation curve, a method for evaluating DKth using a nonlinear function is proposed. It is shown that the proposed method reduces the artificial conservativeness induced by the evaluation method as well as the susceptibility to scatter in test data and the influence of test data density. KW - Fatigue crack propagation threshold KW - ISO 12108 KW - ASTM E647 KW - Data evaluation methods KW - Experimental determination PY - 2022 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-552153 DO - https://doi.org/10.3390/ma15144737 SN - 1996-1944 VL - 15 IS - 14 SP - 1 EP - 21 PB - MDPI CY - Basel AN - OPUS4-55215 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Duarte, Larissa A1 - Madia, Mauro A1 - Zerbst, Uwe T1 - The effect of the environmental conditions on the threshold against fatigue crack propagation N2 - The threshold against fatigue crack propagation (ΔKth) is a crucial parameter for the damage tolerance assessment of engineering components subjected to cyclic loading and it is composed by two distinct components, one intrinsic, dependent on the elastic material properties and the lattice type, and one extrinsic, related to the occurrence of crack closure effects. An important issue is that several factors can influence ΔKth and, in general, the fatigue crack propagation behavior. In this work, the influence of the experimental procedure, air humidity, stress ratio and test frequency on da/dN-ΔK data has been investigated. Results are discussed with their potential causes and consequences on the calculations of the residual lifetime. KW - Fatigue crack propagation threshold KW - Crack closure effect KW - Experimental procedure KW - Environmental conditions PY - 2022 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-544905 DO - https://doi.org/10.1016/j.prostr.2022.03.030 VL - 38 SP - 292 EP - 299 PB - Elsevier B.V. AN - OPUS4-54490 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Duarte, Larissa A1 - Zerbst, Uwe A1 - Madia, Mauro T1 - Vergleichende Untersuchungen zum intrinsischen Schwellenwert der da/dN-ΔK-Kurve N2 - Für die Bestimmung der Restlebensdauer zyklisch beanspruchter Bauteile kommt dem Schwellenwert für Ermüdungsrissausbreitung, Δ𝐾𝑡ℎ, und dem sich anschließenden Schwellenwertbereich der 𝑑𝑎𝑑𝑁⁄−Δ𝐾-Kurve große Bedeutung zu. Dem stehen Unsicherheiten bei der Bestimmung und Analyse gegenüber. Der Aufsatz befasst sich mit der Ermittlung des sogenannten intrinsischen Schwellenwerts, der als robuster Eingangsparameter für eine „rissschließfreie“ Analyse der Restlebensdauer von entscheidender Bedeutung ist. T2 - 53. Tagung des DVM-Arbeitskreises Bruchmechanik und Bauteilsicherheit CY - Online meeting DA - 18.02.2021 KW - Schadenstolerante Bauteilauslegung, Restlebensdauer, intrinsischer Schwellenwert gegen Ermüdungsrissausbreitung PY - 2021 SN - 2366-4797 SP - 211 EP - 220 PB - Deutscher Verband für Materialforschung und -prüfung e.V. (DVM) CY - Berlin AN - OPUS4-52704 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Duarte, Larissa A1 - Zerbst, Uwe A1 - Madia, Mauro T1 - Der Schwellenwert der da/dN-∆K-Kurve als Auslegungskriterium für die Bauteilbewertung N2 - Für die Bestimmung der Restlebensdauer zyklisch beanspruchter Bauteile kommt dem Schwellenwert für Ermüdungsrissausbreitung ∆Kth und dem sich anschließenden Schwellenwertbereich der da/dN-∆K-Kurve große Bedeutung zu. Dem stehen Unsicherheiten bei der Bestimmung und Analyse gegenüber. Der Aufsatz befasst sich mit der Ermittlung des sogenannten intrinsischen Schwellenwerts, der als robuster Eingangsparameter für eine „rissschließfreie“ Analyse der Restlebensdauer von entscheidender Bedeutung ist. T2 - Tagung Werkstoffprüfung 2020 CY - Online meeting DA - 03.12.2020 KW - Schadenstolerante Bauteilauslegung, KW - Intrinsischer Schwellenwert gegen Ermüdungsrissausbreitung KW - Restlebensdauer PY - 2020 DO - https://doi.org/10.48447/WP-2020-025 SP - 1 EP - 8 AN - OPUS4-52788 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER -