TY - CONF A1 - Jaunich, Matthias A1 - Grelle, Tobias A1 - Wolff, Dietmar T1 - Influence of partial release on sealing performance of elastomer O-rings at low temperatures N2 - For many sealing applications rubbers are applied due to their special material properties and easy use. In many applications as e.g. in aviation, traffic or process technology the material can be exposed to low temperatures during operation. Therefore it is important to know the material behaviour at those low temperatures to determine the temperature range that allows a safe operation of the seal. As rubbers are used as main sealing materials for containers for low and intermediate level radioactive waste and as additional component to metal seals in spent fuel and high acitve waste containers, a comprehensive elastomer investigation program is run at BAM. This program comprises investigations of elastomer overall performance, durability, influence of gamma irradiation and low temperature behaviour. In this paper we focus on the behaviour of elastomer seals below ambient temperatures after a fast partial release. Despite the primarily static application conditions of many seals their behaviour after partial compression release is of interest with regard to potential decrease of leak-tightness. For this investigation a special setup was designed which allows the partial release of compressed seal systems at different temperatures accompanied by leakage rate measurements. The results for FKM seals are presented and discussed. T2 - Technomer 2015 - 24. Fachtagung über Verarbeitung und Anwendung von Polymeren CY - Chemnitz, Germany DA - 12.11.2015 KW - O-ring KW - Glass-rubber transition KW - Compression set KW - Partial release PY - 2015 SN - 978-3-939382-12-6 SP - P 3.7, 1 EP - 6 CY - Chemnitz AN - OPUS4-35130 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - An update on metal seal tests performed at BAM and implications for interim storage N2 - The investigation of the long-term performance of sealing systems employed in containers for radioactive waste and spent nuclear fuel is one research focus area for division 3.4 “Safety of Storage Containers” at the Bundesanstalt für Materialforschung und -prüfung. Metallic seals are in use in interim storage casks for used fuel and high active waste. Their change in performance over time is of high importance for maintaining safe enclosure. Therefore, investigations on these systems were started at BAM to get a general understanding of the relevant processes. Our investigations comprise investigations on different parameters which influence the seal performance and the main part is focussed on the time and temperature dependent behaviour. In this contribution an update on the performed tests and their respective results will be given in respect to the overview presented in 2020. The understanding of the long-term behaviour of the sealing systems and the performance evaluation during interim storage and subsequent transportation are our goals. T2 - SEDS-Workshop: Sicherheit der längerfristigen trockenen Zwischenlagerung CY - Garching, Germany DA - 15.05.2024 KW - Metal seals KW - Ageing KW - Leakage rate KW - Creep PY - 2024 AN - OPUS4-60640 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - Investigations on the low temperature performance of rubber seals N2 - For many sealing applications rubbers are applied due to their special material properties and easy use. In many applications as e.g. in aviation, traffic or process technology the material can be exposed to low temperatures during operation. Therefore, it is important to know the material behaviour at those low temperatures to determine the temperature range that allows a safe operation of the seal. In this work, we focus on the behaviour of elastomer seals at low temperatures with regard to potential decrease of leak-tightness or catastrophic seal failure of O-ring rubber seals. This is required as material properties of rubbers are strongly temperature dependent but their temperature application range is not always clearly defined. Based on previous investigations which considered the physical material properties and the seal behaviour under purely static conditions we widen the focus on the sealing performance after a fast partial relief of compressed seals and additional materials. For the investigations, different typical rubber seal materials were used as e.g. fluorocarbon (FKM), ethylene propylene diene (EPDM) and hydrogenated acrylonitrile-butadiene (HNBR) rubber. The correlation of the physical material properties with seal performance is studied. This includes as well purely static sealing applications as the Performance during/after fast partial relief of seals at low temperatures. T2 - Technomer 2017 CY - Chemnitz, Germany DA - 09.11.2017 KW - Seal KW - Rubber KW - Low temperature KW - Recovery PY - 2017 AN - OPUS4-42839 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Jaunich, Matthias A1 - Wolff, Dietmar T1 - Influence of gamma irradiation on low temperature properties of rubber seal materials N2 - In many fields the function of seal materials is required at low temperatures. Therefore the understanding of failure mechanisms at low temperatures is of high importance. In some applications elastomeric seals are used in environments with increased irradiation backgrounds, as e.g. in containers for radioactive waste. This paper reports on the influence of gamma irradiation on the low temperature properties of different fluorocarbon rubber (FKM) materials. The samples were irradiated with gamma doses of up to 600 kGy and the induced changes of material properties were tested by methods sensitive to the rubber-glass transition, like DSC and DMA. Additionally, compression set measurements were performed to give information about recovery behaviour at low temperatures. KW - Seal KW - O-ring KW - Low temperature KW - Gamma irradiation KW - Compression set KW - Dichtungen KW - O-Ringe KW - Tiefe Temperatur KW - Gamma-Bestrahlung KW - Druckverformungsrest PY - 2015 SN - 0948-3276 SN - 0022-9520 VL - 68 IS - 6 SP - 85 EP - 89 PB - Hüthig CY - Heidelberg AN - OPUS4-33552 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Zaghdoudi, Maha A1 - Kömmling, Anja A1 - Jaunich, Matthias A1 - Wolff, Dietmar T1 - Übersicht über laufende Untersuchungen zur Langzeitalterung von Elastomerdichtungen N2 - Eine Aufgabe des Fachbereichs 3.4 Sicherheit von Lagerbehältern der Bundesanstalt für Materialforschung und -prüfung (BAM) ist es, die Sicherheit von Behältern zur Lagerung von radioaktivem Abfall mit vernachlässigbarer Wärmeentwicklung zu bewerten. Da solche Behälter vor der Entsorgung transportiert und gelagert werden, ist während dieser Zeit ein sicherer Einschluss des radioaktiven Inhalts von größter Bedeutung. Zur Abdichtung dieser Behälter sind Elastomer-O-Ringe weit verbreitet. Um für solche, wie auch für viele andere Anwendungen, eine Voraussage über die Lebensdauer dieser Komponenten treffen zu können, ist es unerlässlich zu verstehen, welchen Einfluss der durch Alterung hervorgerufene Abbau auf Dauer auf die Elastomerdichtungen hat. In einem Langzeittest wurden drei Kautschukarten (EPDM und FKM, die für die Anwendung relevant sind, und HNBR als Vergleich) über mehrere Jahre untersucht. Dabei wurden die Veränderungen der mechanischen Eigenschaften (z. B. Härte und Bruchdehnung) bei vier verschiedenen Alterungstemperaturen (75 °C, 100 °C, 125 °C und 150 °C) sowie das Dichtungsverhalten betrachtet. Um den Einfluss von Vernetzung und Kettenspaltung auf die beobachteten Alterungseffekte zu bestimmen, wurden Messungen zur kontinuierlichen und intermittierenden Druckspannungsrelaxation durchgeführt. Dadurch konnten Erkenntnisse über Kinetik und Mechanismus der Abbaureaktionen gewonnen werden. Zur Einschätzung des Dichtungsverhaltens wurden Durckverformungsrest und Leckagerate gemessen. Die Ergebnisse zeigen, dass die O-Ringe unter statischen Bedingungen auch dann dicht halten, wenn die Werte für Druckverformungsrest, Druckspannungsrelaxation und mechanische Eigenschaften schon auf einen fortgeschrittenen Alterungsabbau hindeuten. Aus diesem Grund wurde ein modifizierter Dichtigkeitsversuch mit einer geringen und schnellen teilweisen Entlastung der Dichtung entwickelt, mit dessen Hilfe sich ein Lebensdauerkriterium bestimmen lässt, das eine Sicherheitsspanne für thermische Schrumpfung und Vibrationen beinhaltet. KW - Alterung KW - O-ring KW - Elastomer Dichtung PY - 2020 SN - 0176-1625 VL - 73 IS - 07-08 SP - 326 EP - 332 PB - Gupta CY - Ratingen AN - OPUS4-51207 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Zaghdoudi, Maha A1 - Kömmling, Anja A1 - Jaunich, Matthias A1 - Wolff, Dietmar A1 - Albouy, P.-A. A1 - Häcker, Ralf A1 - Stock, Daniel T1 - Overview of ongoing research and future prospects on polyethylene neutron shielding materials at bam N2 - The extension of the interim storage period of radioactive waste before disposal will cause additional challenges for the nuclear waste management in Germany, so that an extensive knowledge of the long-term performance of casks, including their components and inventories, will be required for future extended storage licenses. Ultra-high and high molecular weight polyethylenes ((U)HMW-PE) are used for neutron shielding purposes in casks for storage and transport of spent fuel and high-level waste due to their extremely high hydrogen content. During their service life of several decades as cask components, the PE materials are exposed to neutron and gamma radiation from the radioactive inventory of the casks, mechanical assembling stresses and temperature. All these combined effects affect the material properties of such components which in turn may be crucial for some possible accident scenarios. At the Bundesanstalt für Materialforschung und -prüfung (BAM), the effects of high temperature exposure in combination with subsequent or previous irradiation were investigated with a comprehensive aging program including thermal aging at 125 °C for different aging periods up to 5 years and irradiation with doses ranging from 50 to 600 kGy. This contribution provides an overview of the ongoing research related to the structural changes of (U)HMW-PE induced by gamma irradiation and high temperature exposure and focuses on current research perspectives at BAM with regard to the prediction of the dynamic behavior of the material during extended interim storage in case of an accident scenario. First results of the coupled effect of temperature, radiation and mechanical loading will be presented. The effect of microstructural changes induced by gamma irradiation and high temperature on the mechanical behavior of (U)HMW-PE will be assessed. T2 - PATRAM22 CY - Juan-Les-Pins, Antibes, France DA - 11.06.2023 KW - (U)HMWPE KW - Ageing KW - Irradiation KW - WAXD KW - SHPB PY - 2023 SP - 1 EP - 10 AN - OPUS4-57707 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Jaunich, Matthias A1 - Probst, Ulrich A1 - Schulz, Sebastian A1 - Wolff, Dietmar A1 - Stark, Wolfgang ED - Berger, K.-F. ED - Kiefer, S. T1 - Elastomere - Untersuchung des Tieftemperaturverhaltens im Dichtungseinsatz N2 - Aufgrund ihrer einfachen und zuverlässigen Anwendung werden Elastomere für viele Dichtungsaufgaben eingesetzt. In vielen Anwendungsbereichen, wie z.B. Verkehr, Luftfahrt und Verfahrenstechnik, können während des Einsatzes tiefe Temperaturen auftreten, bei denen die Funktionsfähigkeit der Dichtung erhalten bleiben muss. Daher ist die Untersuchung des Verhaltens von Elastomerdichtungen bei tiefen Temperaturen wichtig, um ihren Temperatureinsatzbereich nach unten abzugrenzen und dadurch einen verlässlichen Betrieb zu sichern. Ziel dieser Arbeit ist es, den sicheren Einschluss von gefährlichen Gütern unter verschiedenen Umgebungsbedingungen und über lange Zeiten zu ermöglichen bzw. die Materialauswahl entsprechend zu steuern. KW - Dichtung KW - Druckverformungsrest KW - Elastomer KW - Glasübergang PY - 2013 SN - 978-3-9811509-7-1 SP - 82 EP - 91 CY - Mannheim AN - OPUS4-29661 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - Untersuchung des Tieftemperaturverhaltens von Elastomeren im Dichtungseinsatz T2 - Polymerwissenschaftliches Seminar des Fachgebietes Polymertechnik/-physik der TU-Berlin CY - Berlin, Germany DA - 2009-12-02 PY - 2009 AN - OPUS4-20630 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Jaunich, Matthias T1 - The average number of references per article published in Polymer Testing over the years N2 - This Editorial is focussed on the changes in the number of references per article published in Polymer Testing from 1980 until today. To set in into context with other changes a comparison with the impact factor of Polymer Testing is presented. KW - Reference KW - Editorial KW - Impact factor KW - Changes with time PY - 2018 DO - https://doi.org/10.1016/j.polymertesting.2018.05.034 SN - 0142-9418 VL - 68 SP - A1 EP - A2 PB - Elsevier AN - OPUS4-45212 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - Härtung von Harnstoffformmassen: Die Aussagekraft des Kochversuchs! T2 - 10th International AVK Conference on Reinforced Plastics CY - Stuttgart, Germany DA - 2007-11-05 PY - 2007 AN - OPUS4-16089 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Jaunich, Matthias A1 - Stark, Wolfgang T1 - Einfluss der Härtung auf die Materialeigenschaften eines Harnstoffharzes N2 - Über die in der Technik weit verbreitete typisierte Harnstoffformmasse UF 131.5, ein Aminoplast, wird berichtet, dass sie im Zuge der thermisch aktivierten Vernetzungsreaktion wegen "Überhärtung" mangelhafte Eigenschaften annimmt. Zur Verifizierung dieses Effektes werden mithilfe der Ultraschall-Prozesskontrolle gezielt Proben unterschiedlicher Aushärtegrade hergestellt. Sie werden mit verschiedenen Methoden, wie der "Kochprobe" und der Thermoanalyse, charakterisiert und auf ihre Materialeigenschaften untersucht. Dabei zeigt sich ein deutlicher Einfluss der Härtezeit auf die Glasübergangstemperatur der Formmasse. In den mechanischen Eigenschaften ist eine Veränderung allerdings nur in der Schlagzähigkeit festzustellen, die sich mit steigender Härtezeit sogar wesentlich verbessert. PY - 2009 SN - 0025-5300 VL - 51 IS - 11-12 SP - 828 EP - 834 PB - Hanser CY - München AN - OPUS4-20566 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - Influence of partial release on sealing performance of elastomer O-Rings at low temperatures T2 - Technomer 2015 CY - Chemnitz DA - 2015-11-12 PY - 2015 AN - OPUS4-34935 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - Approach for the Investigation of Elastomer Seal long termin Behavior for Transport and Storage Packages T2 - Delft, Netherlands DA - 2014-05-26 PY - 2014 AN - OPUS4-30668 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - Low temperature properties of rubber seals T2 - 9. Rubber Fall Colloquium CY - Hanover, Germany DA - 2010-11-03 PY - 2010 AN - OPUS4-21207 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias A1 - Goral, Milan A1 - Sagradov, Ilja A1 - Wolff, Dietmar A1 - Völzke, Holger T1 - Aging investigations of metal seals used in containers for interim storage of spent fuel N2 - For bolted casks for used fuel and high level waste the sealing system has an important impact of ensuring safe enclosure of the inventory The used metal seals show some changes over time which have been addressed for nearly 15 years in running experiments at BAM The observed changes are temperature de pendent and therefore it is expected that test s at higher temperature allow for an acceleration of the effects and ideally the proposal of an ageing model covering the expected time of use . Nevertheless, questions concerning the influence of the experimental approach on the results and effects taking place at the initial days of ageing remain. To address these a new project was launched to give a better understanding of the seal behavior. T2 - PVP2024, Pressure Vessels & Piping Conference CY - Bellevue, WA, USA DA - 29.07.2024 KW - Metal seal KW - Aging KW - Interim storage PY - 2024 SN - 978-0-7918-8851-3 SP - 1 EP - 4 PB - ASME AN - OPUS4-61357 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - Tests of metallic seals at Bam 3.4 performed over more than 15 years N2 - The investigation of the long-term performance of sealing systems employed in containers for radioactive waste and spent nuclear fuel is one research focus area for division 3.4 “Safety of Storage Containers” at the Bundesanstalt für Materialforschung und -prüfung (BAM) in Germany. The time dependant behaviour of metallic seals, which are employed in interim storage casks for used fuel and high active waste, is of high importance for ensuring safe enclosure. Therefore, investigations on these systems were started at BAM to get a general understanding of the relevant processes. Our investigations comprise investigations on different parameters which influence the seal performance and the main part is focussed on the time and temperature dependent behaviour. In this contribution an overview of the performed tests and their respective results will be given. T2 - 5th sealing workshop by Maestral CY - Avignon, France DA - 05.11.2024 KW - Metal seal KW - Aging KW - Interim storage PY - 2024 AN - OPUS4-62048 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - Überwachung des Vulkanisationsverlaufs mit Ultraschall T2 - Jahrestagung der Deutschen Kautschuk-Gesellschaft (DKG), Bezirksgruppe Ost CY - Bad Lauchstädt, Germany DA - 2007-11-08 PY - 2007 AN - OPUS4-16088 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias A1 - Hagenow, Peter A1 - Kasparek, Eva Maria A1 - Kömmling, Anja A1 - Noack, Volker A1 - Völzke, Holger A1 - Wolff, Dietmar T1 - Requirements for the use of elastomer seals in casks for final disposal of low and intermediate level waste N2 - Elastomer seals are widely used as barrier seals in containers for low and intermediate level radioactive waste and in some countries for spent fuel transportation casks. Depending on the area of use, the rubber materials have to demonstrate proper sealing performance with regard to mechanical, thermal and environmental conditions as well as irradiation during the entire operation period. In Germany the low and intermediate level radioactive waste is planned to be disposed in the Konrad repository in standardized containers. Many of these containers use an elastomer seal between lid and container body. Depending on the radiactive inventory and a possible containment of the waste in inner barrels and/or concrete structures, such containers may require a specific leak tightness. In such cases, specified leakage rates are shall not be exceeded by the the seals to keep potential activity releases from the inventories well below defined limits. Generally, all waste containers have to fulfill the waste acceptance criteria for the Konrad repository as defined by the reports BfS SE-IB-29/08 and SE-IB-30/08. From these criteria several requirements for seal performance are derived. The seals have to: - ensure full functionality until final container disposal, - maintain its function in case of a thermal or mechanical accident, - ensure encapsulation also at -20 °C. This combination of requirements is challenging especially as a seal exchange, which is typical for many other applications, is hardly possible and thus a sound understanding of how to perform safety evaluation of containers is required. Therefore BAM has initiated investigations on elastomer seal behaviour. This work focuses on low temperature behaviour and sealing performance concerning static conditions as well as partial loss of compression and ageing of elastomer seals. Concerning ageing, property changes caused by long-term thermooxidative conditions as well as gamma irradiation are investigated. This contribution presents an overview and explanation of the aims of the ongoing research and gives an update of the most relevant results. T2 - 13th Internationales Symposium "Konditionierung radioaktiver Betriebs- und Stillegungsabfälle CY - Dresden, Germany DA - 22.03.2017 KW - Disposal KW - Konrad repository KW - Seal PY - 2017 SP - 595 EP - 601 AN - OPUS4-39870 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Kömmling, Anja A1 - Jaunich, Matthias A1 - Pourmand, P. A1 - Wolff, Dietmar A1 - Gedde, U.W. T1 - Influence of ageing on sealability of elastomeric O-rings N2 - At BAM, which is the federal institute for materials research and testing in Germany, it is one of our tasks to evaluate the safety of casks designed for transport and/or storage of radioactive material. This includes the assessment of the service lifetime of elastomeric seals that are part of the container lid system with regard to the requirements for long-term safety (40 years and more) of the containers. Therefore, we started an accelerated ageing programme with selected rubbers often used for seals (HNBR, EPDM and FKM) which are aged at four different temperatures (75 °C, 100 °C, 125 °C and 150 °C) up to 1.5 years. In order to assess sealability, O-rings are aged in compression by 25 % (corresponding to the compression during service) between plates as well as in flanges that allow leakage rate measurements. For comparison, uncompressed O-rings are aged as well. Further methods characterising seal performance are compression stress relaxation (CSR) reflecting the loss of sealing force of a compressed seal over time, and compression set (CS) which represents the recovery behaviour of a seal after release from compression. Additionally, hardness is measured for information about the change of mechanical properties. The experimental results indicate that while hardness, CSR and CS show considerable degradation effects, the leakage rate stays relatively constant or even decreases until shrinkage combined with the loss of resilience of the aged seal leads to leakage. This demonstrates that static leakage rate, which is the only available direct seal performance criterion, has only limited sensitivity towards the degradation of the seal material. CS data is extrapolated using time-temperature shifts and Arrhenius graphs. An exemplary CS of 50 % would be reached after approx. 1.2, 17 and 29 years at 60 °C for HNBR, EPDM and FKM respectively. T2 - PolymerTec 2016 CY - Merseburg, Germany DA - 15.06.2016 KW - Compression KW - Leakage KW - Degradation KW - Rubber KW - Lifetime PY - 2017 DO - https://doi.org/10.1002/masy.201600157 SN - 1022-1360 SN - 1521-3900 VL - 373 IS - 1 SP - UNSP 1600157, 1 EP - 10 PB - WILEY-V C H VERLAG GMBH CY - Weinheim AN - OPUS4-40958 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Kömmling, Anja A1 - Jaunich, Matthias A1 - Wolff, Dietmar T1 - Ageing of elastomeric seals for storage containers N2 - At BAM Federal Institute for Materials Research and Testing in Germany, it is our responsibility to evaluate the safety of casks designed for transport and/or storage of radioactive material. This includes the investigation of elastomeric seals applied in the containers. Besides examining the low-temperature behavior of elastomeric seals, it is our goal to evaluate the service lifetime of the seals with regard to the requirements for long-term safety (40 years and more) of the containers. Furthermore, we deem it necessary to exceed the requirements given in the ageing standard DIN 53508 and take into account diffusion-limited oxidation (DLO) effects and non-Arrhenius behavior when making lifetime predictions. Therefore, we started an ageing programme with selected rubbers (HNBR, FKM and EPDM) which are oven-aged at four different temperatures (75 °C, 100 °C, 125 °C and 150 °C) in order to extrapolate the data to service temperature using different models and check which one is appropriate. Samples are examined at different times up to 5 years. In order to be able to compare between compressed and relaxed rubber, they are aged in two conditions: the undeformed O-ring state as well as compressed between plates with a compression of 25 % corresponding to the actual compression during service. Additionally, we are ageing samples in flanges that allow leakage rate measurements which is the central performance criterion. Analysis methods include hardness as a quick indicator, compression set and compression stress relaxation as measures reflecting the actual properties of a compressed seal. Additionally, we are applying classical polymer analysis methods like dynamic mechanic analysis and thermogravimetric analysis which show changes in the polymeric structure due to chain scission and crosslinking. Furthermore, we are testing the leakage rate of the O-rings in order to correlate the changes in physical properties to the actual performance of the seal. First results of samples aged up to 100 days show a strong increase in hardness for HNBR, a moderate increase for EPDM and hardly a change for FKM. A similar result is seen in the compression set of samples aged 100 d at 100 °C in compression as HNBR has reached 60 %, EPDM 25 % and FKM 15 % compression set. However, after ageing at 150 °C, EPDM shows a worse performance with 95 % compression set compared to HNBR with only 80 %. This is probably due to DLO effects in HNBR that appear because of the fast ageing and low oxygen permeability in HNBR. This leads to a deficit of oxygen in the center of the sample which is thus protected from ageing and can retain elastic properties. The full paper shall discuss the changes in material properties observed to date and the impact on the performance of elastomeric seals. T2 - IRC 2015 - International rubber conference CY - Nürnberg, Germany DA - 29.06.2015 KW - Elastomer KW - Rubber KW - Aging KW - Lifetime KW - Seal KW - Cask KW - Compression PY - 2015 SP - 1 EP - 10 AN - OPUS4-34939 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Wolff, Dietmar A1 - Jaunich, Matthias A1 - Stark, Wolfgang T1 - Investigating the performance of rubber seals at low temperatures N2 - Rubbers are widely used as main sealing materials for Containers for low and intermediate level radioactive waste and as additional component to metal seals in spent fuel and high active waste containers. The save enclosure of the radioactive container inventory has to be guaranteed according to legislation and appropriate guidelines for long term storage periods as well as down to temperatures of -40 °C for transportation. Therefore the understanding of failure mechanisms that lead to leakage at low temperatures is necessary to ensure a proper material choice which is certainly also influenced by additional factors as e.g. the aging behavior. T2 - 14th International high-level radioactive waste management conference CY - Albuquerque, New Mexico, USA DA - 28.04.2013 KW - Rubber seals KW - Elastomers KW - Compression set KW - Low temperature KW - Leakage rate PY - 2013 SN - 978-1-62748-644-6 SP - 1 EP - 7(Paper # 6888) PB - Omnipress AN - OPUS4-28530 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - O-ring seals: Material degradation, seal performance and determination of end-of-lifetime criterion N2 - Ageing of O-ring seals to evaluate the probable lifetime is an important task for long term applications. In this contribution the material degradation of O-ring seals is studied and a suitable end-of-lifetime criterion is determined under consideration of the application conditions. T2 - VDI Fachtagung Dichtungstechnik CY - Schweinfurt, Germany DA - 27.06.2017 KW - O ring KW - Ageing KW - Lifetime criterion PY - 2017 AN - OPUS4-40957 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Kömmling, Anja A1 - Jaunich, Matthias A1 - Goral, Milan A1 - Wolff, Dietmar T1 - Insights for lifetime predictions of O-ring seals from five-year long-term aging tests N2 - O-rings made of HNBR, EPDM and FKM were aged in the compressed and uncompressed state at 150 °C, 125 °C, 100 °C, 75 °C, 60 °C and 23 °C for aging times of up to five years. Hardness was measured and increased with aging time and temperature for HNBR and EPDM, but it remained practically constant for FKM. Indenter modulus measurements were performed on the lateral O-ring surface (that was free of DLO effects) to assess an influence of the compression during aging, but none was detected. The equilibrium compression set (CS) exhibited faster and stronger degradation than hardness and was used for lifetime predictions using the time-temperature superposition (TTS) principle. With an end-of-lifetime criterion of 70 % CS, lifetimes of 4.5 years, 50 years and 526 years at 75 °C were estimated for HNBR, EPDM and FKM, respectively. The activation energies derived from an Arrhenius plot of the shift factors from the TTS were 85 kJ/mol, 99 kJ/mol and 78 kJ/mol for HNBR, EPDM and FKM, respectively, revealing that a higher activation energy does not necessarily mean that the material has a higher lifetime at lower temperatures. Furthermore, the measured lifetime of EPDM O-rings at 100 °C (5 years) was compared to that predicted on the basis of the lifetime at 150 °C as well as 125 °C using the corresponding shift factors. The error of the prediction was only ± 4 %. However, this precise prediction could only be achieved using the five-year long-term aging data. When using only data from aging times up to 0.5 years and 2 years, the lifetime of EPDM O-rings at 100 °C was underestimated by 31 % and 22 %, respectively. KW - HNBR KW - EPDM KW - FKM KW - DLO KW - Hardness KW - Compression set KW - Rubber KW - Elastomer KW - Degradation PY - 2020 DO - https://doi.org/10.1016/j.polymdegradstab.2020.109278 VL - 179 SP - 109278 PB - Elsevier Ltd. AN - OPUS4-51060 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias A1 - Kömmling, Anja A1 - Horn, Jutta A1 - Völzke, Holger A1 - Wolff, Dietmar T1 - Long-Term Performance of Elastomer seals - From Aging Tests to Lifetime Estimations N2 - Elastomers show a high versatility which makes them ideal materials for sealing applications in various fields. Especially under changing application conditions the high recovery potential of this class of material is beneficial to compensate temperature or pressure fluctuation, and geometrical changes resulting from mechanical loads in e.g. accident conditions. Out of these reasons elastomers are also used in containers for low and intermediate level radioactive waste and for spent fuel transportation casks. In casks designed for low and intermediate level waste elastomer seals can act as primary seal responsible for the containment function whereas in spent fuel storage and transportation casks (dual purpose casks (DPC)) elastomer seals are used as auxiliary seals to allow leakage rate measurements of metal barrier seals. An inherent prerequisite for this kind of application is the Long time-scale of operation without or with limited possibility of seal replacement. In Germany an interim storage license for DPC`s is typically issued for 40 years, a timeframe which might increase in the future due to challenges of the final repository siting procedure. For low and intermediate level waste, also long time periods are required before final disposal can be achieved. Therefore, the performance of elastomer seals over extended time periods is, as for other applications, of high importance. A typical approach to ensure long-term functionality is to perform accelerated aging tests to calculate an estimated lifetime by assuming e.g. Arrhenius like equations for the timetemperature relationship. This approach requires a suitable end of life criterion considering the application of interest. This often can represent a challenge on its own. As BAM is involved in most of the cask licensing procedures and especially responsible for the evaluation of cask-related long-term safety issues we initiated several test programs for investigating the behavior of elastomer seals. Experiments concerning the low temperature performance down to -40 °C and the influence of gamma irradiation have been started first. Currently the thermal aging behavior of elastomer seals, which is the topic of this contribution, is examined. For our aging investigations we use a broad approach to first determine the property changes in different elastomer materials due to thermo-oxidative aging at elevated temperatures and secondly, we test how the typical methods of lifetime extrapolation can be applied to these results. This Approach enables us to detect and exclude undesired side effects which very often influence lifetime estimations. In this contribution, our recent results are extended. The results show that lifetime estimation based on single material properties can be misleading and therefore a combination of several methods is recommended. T2 - ASME 2018 Pressure Vessels and Piping Conference CY - Prague, Czech Republic DA - 15.07.2018 KW - Seal performance KW - Rubber KW - Ageing PY - 2018 VL - PVP2018 SP - 84631-1 EP - 84631-8 AN - OPUS4-46346 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Zaghdoudi, Maha A1 - Kömmling, Anja A1 - Jaunich, Matthias A1 - Wolff, Dietmar T1 - Erroneous or Arrhenius: A Degradation Rate-Based Model for EPDM during Homogeneous Ageing N2 - To improve the predictive capability of long-term stress relaxation of elastomers during thermo-oxidative ageing, a method to separate reversible and irreversible processes was adopted. The separation is performed through the analysis of compression set after tempering. On the Basis of this separation, a numerical model for long-term stress relaxation during homogeneous ageing is proposed. The model consists of an additive contribution of physical and chemical relaxation. Computer simulations of compression stress relaxation were performed for long ageing times and the results were validated with the Arrhenius treatment, the kinetic study and the time-temperature superposition technique based on experimental data. For chemical relaxation, two decay functions are introduced each with an activation energy and a degradative process. The first process with the lower activation energy dominates at lower ageing times, while the second one with the higher activation energy at longer ageing times. A degradation-rate based model for the evolution of each process and ist contribution to the total system during homogeneous ageing is proposed. The main advantage of the model is the possibility to quickly validate the interpolation at lower temperatures within the range of slower chemical processes without forcing a straight-line extrapolation. KW - Kinetic study KW - Arrhenius KW - TTS KW - Modeling KW - Chemical processes KW - Stress relaxation PY - 2020 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-512931 DO - https://doi.org/10.3390/polym12092152 SN - 2073-4360 VL - 12 IS - 9 SP - 1 EP - 21 AN - OPUS4-51293 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Goral, Milan A1 - Kömmling, Anja A1 - Probst, Ulrich A1 - Wossidlo, Peter A1 - Jaunich, Matthias A1 - Wolff, Dietmar A1 - Völzke, Holger T1 - Langzeitversuche über 10 Jahre an Federkern-Metalldichtungen mit Aluminium- bzw. Silberummantelungen N2 - Federunterstützte Metalldichtungen mit Aluminium(Al)- oder Silber(Ag)-Ummantelung werden u.a. in Behältern für Wärme entwickelnde radioaktive Abfälle eingesetzt, da diese Dichtungen eine sehr gute Dichtheit gewährleisten sowie Langlebigkeit und Beständigkeit gegenüber erhöhten Temperaturen und radioaktiver Strahlung aufweisen. Auch wenn die Sicherheit solcher Behälter und der verwendeten Dichtungen vielfach belegt wurde, sind sie Gegenstand andauernder Forschung, etwa im Hinblick auf eine absehbar benötigte verlängerte Zwischenlagerdauer. Aus diesem Grund werden an der Bundesanstalt für Materialforschung und -prüfung (BAM) im Fachbereich 3.4 „Sicherheit von Lagerbehältern“ seit über 20 Jahren Versuche an solchen Metalldichtungen durchgeführt. Dabei sollen zusätzliche Erkenntnisse hinsichtlich der Sicherheitsreserven der Dichtungen in unterstellten Störfallszenarien (axiale Bewegung des Deckelsystems bzw. Aufweitung der Nutgeometrie) und insbesondere detailliertere Erkenntnisse zum Langzeitverhalten gewonnen werden. KW - Federunterstützte Metalldichtungen KW - Transport- und Lagerbehälter für radioaktive Stoffe KW - Langzeitversuche KW - Alterung KW - Dichtheit KW - Leckagerate KW - Helium-Dichtheitsprüfung PY - 2023 VL - 2023 SP - 43 EP - 63 PB - ISGATEC GmbH CY - Mannheim AN - OPUS4-56399 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Grelle, Tobias A1 - Wolff, Dietmar A1 - Probst, Ulrich A1 - Jaunich, Matthias A1 - Völzke, Holger T1 - Investigation programme for evaluation and prediction of the long-term behaviour of Helicoflex® metal seals N2 - In Germany, for the transport and storage of spent nuclear fuel, casks with double closure lid systems are used, which are equipped with Helicoflex® metal seals. The original interim storage period for these casks was planned to be 40 years. However, recent political developments indicate that a storage time of more than 80 years might be necessary. Therefore, the current storage licenses have to be renewed in due course, which requires extended knowledge of the long-term behaviour of all cask components. At the Bundesanstalt für Materialforschung und -prüfung (BAM), metal seals have been investigated after ageing at temperatures between room temperature and 150 °C for up to 7 years. At regular intervals the seals have been tested for leakage rate as well as for their mechanical behaviour. From these tests pronounced influence of ageing could be shown which results in the decrease of the seal force and the useable resilience. The main reason attributed to these performance changes is the increasing permanent deformation of the outer layer of the seal due to creep. So far, an explicit analytical description of the long-term behaviour that could be used for predictions exceeding the tested ageing times and temperatures was not suitable. In addition to the component tests that were already conducted, a comprehensive investigation programme has been started to describe the mechanical behaviour of the individual seal components. The individual seal components are tested regarding different material characteristics including creep, deformation and microstructural properties. The comparability of the material characterization is ensured by comparing the basic raw material of the specimen with the actual component material. Furthermore, detailed investigations of the time and temperature dependent deformation behaviour are realized by ageing seal segments at multiple temperatures for different periods of time and employing standardized tests. By analysing the acquired data in combination with the ongoing long-term component tests a dataset for analytical prediction of the long-term behaviour of the seals is intended for an extended period of time under a certain temperature regime. T2 - 48th Annual Meeting on Nuclear Technology (AMNT 2017) CY - Berlin, Germany DA - 16.05.2017 KW - Metal seal KW - Creep KW - Long-term behavior PY - 2017 SP - 1 EP - 7 AN - OPUS4-43418 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Grelle, Tobias A1 - Wolff, Dietmar A1 - Probst, Ulrich A1 - Jaunich, Matthias A1 - Völzke, Holger T1 - Material investigation and long-term sealing behavior of Helicoflex® metal seals used in containers for spent nuclear fuel N2 - In Germany spent nuclear fuel is stored and transported in casks that possess bolted lid systems equipped with double jacket metal seals of Helicoflex® type in order to enable safe enclosure of the radioactive inventory. A dry interim storage period of 40 years was planned and the casks are licensed for that time span. However, due to political reasons and delayed disposal projects this time span is expected to increase significantly. It is therefore necessary to evaluate the long-term sealing behavior of the casks exceeding 40 years of operating time. In this paper, we discuss our approach to investigate the aging behavior of such metal seals, and to predict the long-term sealing behavior. Accelerated aging component tests with seals are performed at temperatures up to 150°C to investigate the course of seal force, useable resilience and leakage rate. Even though these tests have already shown a significant decrease in seal force and useable resilience after aging times of less than 1 year, for most seals the leakage rate stayed better than the specified value. However, observation of the leakage rate has to be continued to determine the aging effect on the seal properties. As a main influence on the seal long-term behavior the increasing permanent deformation of the outer jacket has been recognized. It is made of aluminum or silver which means that the temperatures that are relevant for the aforementioned application in casks lead to creep deformation. For further investigation of seal behavior a comprehensive research program concerning the material characteristics and aging behavior of the individual seal components, with an emphasis on the outer jacket material, has been launched. The aim is to get a better understanding of the time and temperature dependent creep mechanisms and deformation. The examinations are separated into tests on seal segments and tests on standardized specimen. In order to be able to study the aging process, seal segments are compressed in flanges and stored at temperatures ranging from room temperature to 150°C. After defined time intervals the segments are analyzed by using standardized tests including structure investigation and creep tests. The results are compared with the behavior of the specimen basic raw material. This is done to ensure comparability of the thin jacket material and additional sheet material used for standardized tests. Thus, the prediction of component changes after different aging times at different temperatures can be made. As a result forecasts on the long term seal behavior are intended. T2 - Waste Management Symposia CY - Phoenix, AZ, USA DA - 05.03.2017 KW - Metal seal KW - Creep KW - Long-term behavior PY - 2017 SN - 978-0-9828171-6-2 SP - Article 17135, 1 EP - 8 AN - OPUS4-40611 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Kömmling, Anja A1 - Chatzigiannakis, E. A1 - Beckmann, Jörg A1 - Wachtendorf, Volker A1 - von der Ehe, Kerstin A1 - Braun, Ulrike A1 - Jaunich, Matthias A1 - Schade, U. A1 - Wolff, Dietmar T1 - Discoloration Effects of High-Dose gamma-Irradiation and Long-Term Thermal Aging of (U) HMW-PE N2 - Two polyethylene types with ultra-high (UHMWPE) and high molecular weight (HMW-PE) used as neutron radiation shielding materials in casks for radioactive waste were irradiated with doses up to 600 kGy using a 60Co gammasource. Subsequently, thermal aging at 125∘C was applied for up to one year. Degradation effects in the materials were characterized using colorimetry, UV-Visspectroscopy, IR spectroscopy, and DSC. Both materials exhibited a yellowing upon irradiation.The discoloration of UHMW-PE disappeared again after thermal aging.Therefore, the yellowing is assumed to originate fromannealable color centers in the formof free radicals that are trapped in the crystalline regions of the polymer and recombine at elevated temperatures. For the antioxidantcontaining HMWPE, yellowing was observed after both irradiation and thermal aging. The color change was correlated mainly to decomposition products of the antioxidant in addition to trapped radicals as in UHMW-PE. Additionally, black spots appeared after thermal aging of HMW-PE. KW - Irradiation KW - UHMWPE KW - Colour center KW - Yellowness index PY - 2017 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-423992 DO - https://doi.org/10.1155/2017/1362491 SN - 1687-9422 VL - 2017 IS - Article ID 1362491 SP - 1 EP - 10 PB - Hindawi AN - OPUS4-42399 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias A1 - von der Ehe, Kerstin A1 - Wolff, Dietmar A1 - Völzke, Holger A1 - Stark, Wolfgang T1 - Understanding the low temperature properties of rubber seals N2 - Rubbers are widely used as main sealing materials for containers for low and intermediate level radioactive waste and as additional component to metal seals in spent fuel and high active waste containers. The save encapsulation of the radioactive container inventory has to be guaranteed according to legislation and appropriate guidelines for long term storage periods as well as down to temperatures of -40 °C during transport. Therefore the understanding of failure mechanisms that lead to leakage at low temperatures is of high importance. It is known that the material properties of rubbers are strongly temperature dependent. At low temperatures this is caused by the rubber-glass transition (abbr. glass transition). During continuous cooling the material changes from rubber-like entropy-elastic to stiff energy-elastic behaviour, that allows nearly no strain or retraction, due to the glass transition. Hence rubbers are normally used above their glass transition but the minimum working temperature limit is not defined precisely, what can cause problems during application. Therefore the lower operation temperature limit of rubber seals should be determined in dependence of the material properties. The results of Differential Scanning Calorimetry (DSC) and Dynamic Mechanical Analysis (DMA) are combined with the results of standardized measurements as the compression set according to ISO 815. To reduce the test time of the standard tests a faster technique was developed. Additionally, the breakdown temperature of the sealing function of complete O-ring seals is measured in a component test setup to compare it with the results of the other tests. The experimental setup is capable of measuring the leakage rate at low temperatures by the pressure rise method. A fluorocarbon rubber (FKM) was selected for this investigation as it is often used for radioactive waste containers. Some materials (seals and test sheets) were purchased from a commercial seal producer and some materials were compounded and cured at BAM in form of rubber sheets. T2 - PATRAM 2010 - 16th International symposium on the packaging and transport of radioactive materials CY - London, UK DA - 2010-10-03 KW - Dichtungen KW - Elastomere KW - Tieftemperaturverhalten PY - 2010 SP - 1 EP - 7 (Session T41 / Paper 169) AN - OPUS4-23887 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Agroui, K. A1 - Jaunich, Matthias A1 - Hadj Arab, A. T1 - Analysis techniques of polymeric encapsulant materials for photovoltaic modules: situation and perspectives N2 - The properties of the encapsulant are critical to the long-term performance of photovoltaic (PV) modules under the influence of sunlight including UV, elevated temperature, humidity and diffusion of oxygen. Encapsulation process represents a bout 40% of the whole PV module cost. The introduction of new non-EVA encapsulant material type "Low-Cost, High-Performance" should provide a solution to outdoor yellowing degradation problems. The emerging encapsulant materials exhibit a good compatibility with emerging PV solar cells for long term durability. This new generation of encapsulant materials has the advantage to improve e the PV module performances and long term durability for specific climate like desert regions. This scientific contribution presents an overview of the different encapsulant materials currently on the market, the general requirements of the emerging encapsulant materials and characterizations techniques for degradation, diagnostic and reliability lifetime estimation in the framework of Algerian renewable energy strategy. T2 - Africa-EU Renewable Energy Re search and Innovation Symposium, RERIS 2016 CY - Tlemcen, Algeria DA - 08.03.2016 KW - Solar cell KW - Polymer encapsulant KW - PV module KW - Encapsulation process KW - Analysis technique PY - 2016 UR - https://nbn-resolving.org/urn:nbn:de:kobv:b43-377186 DO - https://doi.org/10.1016/j.egypro.2016.07.171 SN - 1876-6102 VL - 2016 IS - 93 SP - 203 EP - 210 PB - Elsevier Ltd. AN - OPUS4-37718 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias A1 - Stark, Wolfgang A1 - Wolff, Dietmar T1 - Behaviour of rubber seals at low temperatures - results of component tests - N2 - The investigation of low temperature properties of elastomeric sealing materials by means of thermo-analytical methods is a sound way to get information about the glass transition process. The breakdown temperature of the sealing function of O-ring seals was measured in a component test setup depending on material and degree of compression. An in depth explanation of the observed component tests behaviour is currently in preparation. It requires the results of thermo-analytical methods and measurements as the compression set (not shown here). With that, a model was developed to describe the correlation between physical material parameters and observed component behaviour. T2 - Jahrestagung Kerntechnik 2013 CY - Berlin, Germany DA - 14.05.2013 PY - 2013 SP - 1 EP - 6 AN - OPUS4-28574 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - von der Ehe, Kerstin A1 - Jaunich, Matthias A1 - Böhning, Martin A1 - Goering, Harald A1 - Wolff, Dietmar T1 - Detection of structural changes of (U)HMW-PE induced by gamma irradiation T2 - 14th International conference "Polymeric materials" CY - Halle (Saale), Germany DA - 2010-09-15 PY - 2010 SN - 978-3-86829-282-4 SP - 1 EP - 6 PB - Druck-Zuck GmbH CY - Halle / Saale AN - OPUS4-21997 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - Behaviour of Rubber Seals at Low Temperatures - Results of Component Tests - T2 - Jahrestagung Kerntechnik 2013 CY - Berlin, Germany DA - 2013-05-14 PY - 2013 AN - OPUS4-28519 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - In-situ Vulcanization monitoring by ultrasonic wave propagation T2 - 8. Kautschuk-Herbst-Kolloquium CY - Hanover, Germany DA - 2008-11-26 PY - 2008 AN - OPUS4-19008 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - Aktueller Stand des Forschungsprojekts LaMEP N2 - Ergebnispräsentation zum Forschungsprojekt "Langzeitverhalten von Metall- und Elastomerdichtungen sowie Moderator-materialien als sicherheitsrelevante Komponenten von TLB für radioaktive Stoffe“ (LaMEP). T2 - BGZ Fachworkshop Zwischenlagerung CY - Berlin, Germany DA - 22.10.2019 KW - Metalldichtung KW - Elastomerdichtung KW - Neutronen Abschirmmaterial KW - Alterung KW - Degradation PY - 2019 AN - OPUS4-49429 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Weber, Mike A1 - Jaunich, Matthias A1 - Goral, Milan A1 - Völzke, Holger T1 - Reproducing and discussion of mechanisms in the contact area between metallic seals and flange during aging by finite element analysis (FEA) N2 - When the first site-specific interim storage licenses for DPCs (dual purpose casks), loaded with spent nuclear fuel or vitrified high-level waste from reprocessing were issued, a duration of 40 years was considered for interim storage license application and the long-term safety assessment of casks. In the meantime, the availability of a final repository is further delayed by several decades and thus interim storage for more than a century becomes a necessity. To assess the long-term performance of the typically used metal seals (e.g. Helicoflex), consisting of a helical spring (Nimonic), an inner stainless steel liner and an outer liner made from silver or aluminum, several experimental programs were conducted and are still ongoing. The investigated metal seals are typically mounted in mock-up flange systems and stored at increased temperatures to accelerate the aging process. In certain intervals the remaining seal force, the useable resilience and the corresponding leakage rate are determined. BAM has accompanied such programs for many years and started independent investigations in 2009. Although the remaining seal force is often used as “…one of the key parameters regarding sealing performances over time…” the presented results so far have shown that the courses of the leakage rate and the remaining seal force do not always correlate as expected. In 2016 BAM firstly published results of seals with aluminum liners where the measured leakage rate started to rise after a quite short time period (< 1 year) at 150 °C, although the seal force decreased only slightly compared to the previous measurement. After exceeding the required leakage rate of 10-8 Pa*m3/s it decreased again to acceptable values in the further course of aging. With reference to already published works, BAM has developed a new detailed ABAQUS finite-element (FE) model to represent the behavior of the seal mounted in the mock-up flange during aging, mainly characterized by the creeping of the outer liner. The main goal of the numerical simulation is to reproduce and understand the changing distribution of contact stresses (outer liner/flange) during aging and to discuss if and how it could be causative for the observed early breach of the leak tightness criteria and its later recovery. T2 - PATRAM 2025, 21st International Symposium on the Packaging and Transportation of Radioactive Materials CY - San Antonio, Texas, USA DA - 27.07.2025 KW - Finite element analysis KW - Metallic seals KW - Aging KW - Contact area PY - 2025 SP - 1 EP - 10 PB - INMM CY - Indianopolis, Indiana, USA AN - OPUS4-63882 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias A1 - Kömmling, Anja A1 - Böhning, Martin A1 - Silbernagl, Dorothee T1 - Comparison of ageing behavior of O-ring seals under hydrogen and air N2 - Elastomeric seals are essential components in the infrastructure which prevent leakage of gas and ensure proper function of technical devices and are therefore highly safety relevant. For proper function a remaining resilience and tolerance to pressure changes is required. The ageing of elastomers is an undesirable but inevitable process leading to a limited lifetime of rubber products such as seals. Independent of the application, as e.g. automotive, piping or container applications, a long lifetime or at least a timely exchange of a seal before occurrence of critical failure is desired. Hydrogen is a key element for the energy turnaround and therefore the compatibility of seals with hydrogen is essential. In addition to the effect of hydrogen uptake and release, which might also cause destructive effects such as rapid gas decompression, ageing at high temperature under hydrogen atmosphere is of interest too. Most of the existing work is addressing the performance of new materials and comprises only very limited investigations concerning long-term use and the behaviour of aged materials in contact with hydrogen. As ageing can lead to substantial changes of material properties, it must be evaluated whether these changes are beneficial or deteriorating for the component function. In this work we present and compare results of the characterization of three sealing materials (EPDM, HNBR, FKM) after ageing at high temperature under hydrogen and air. Despite the common assumption that ageing under hydrogen atmosphere should be less severe for the material in comparison to air ageing, this is not the case for every material. T2 - ASME PVP2025, Pressure Vessels & Piping Conference CY - Montreal, Quebec, Canada DA - 20.07.2025 KW - Aging KW - Seal KW - Compression set KW - Atomic force microscopy PY - 2025 SP - 1 EP - 7 AN - OPUS4-63889 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - Investigation of the low-temperature performance of rubber seals N2 - For many sealing applications rubbers are applied due to their special material properties and easy use. In many applications as e.g. in aviation, traffic or process technology the material can be exposed to low temperatures during operation. Therefore, it is important to know the material behaviour at those low temperatures to determine the temperature range that allows a safe operation of the seal. In this work, we focus on the behaviour of elastomer seals at low temperatures with regard to potential decrease of leak-tightness or catastrophic seal failure of O-ring rubber seals. This is required as material properties of rubbers are strongly temperature dependent but their temperature application range is not always clearly defined. Based on previous investigations which considered the physical material properties and the seal behaviour under purely static conditions we widen the focus on the sealing performance after a fast partial relief of compressed seals and additional materials. For the investigations, different typical rubber seal materials were used as e.g. fluorocarbon (FKM), ethylene propylene diene (EPDM) and hydrogenated acrylonitrile-butadiene (HNBR) rubber. The correlation of the physical material properties with seal performance is studied. This includes as well purely static sealing applications as the performance during/after fast partial relief of seals at low temperatures. T2 - Polymertec 2018 CY - Merseburg, Germany DA - 13.06.2018 KW - Seal KW - Low temperature KW - Leakage PY - 2018 AN - OPUS4-45214 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - Comparison of ageing behaviour of O-ring seals under hydrogen and air N2 - Elastomeric seals are essential components in the infrastructure which prevent leakage of gas and proper function of technical devices and are therefore highly safety relevant. For proper function a remaining resilience and tolerance to pressure changes is required. The ageing of elastomers is an undesirable but inevitable process leading to a limited lifetime of rubber products such as seals. Independent of the application, as e.g. automotive, piping or container applications, a long lifetime or at least a timely exchange of a seal before occurrence of critical failure is desired. Hydrogen is a key element for the energy turnaround and therefore the compatibility of seals with hydrogen is essential. In addition to the effect of hydrogen uptake and release, which might also cause destructive effects such as rapid gas decompression, ageing at high temperature under hydrogen atmosphere is of interest too. Most of the existing work is addressing the performance of new materials and comprises only very limited investigations concerning long-term use and the behaviour of aged materials in contact with hydrogen. As ageing can lead to substantial changes of material properties, it must be evaluated whether these changes are beneficial or deteriorating for the component function. In this work we present and compare results of the characterisation of three sealing materials (EPDM, HNBR, FKM) after ageing at high temperature under hydrogen and air. Despite the common assumption that ageing under hydrogen atmosphere should be less severe for the material in comparison to air ageing, this is not the case for every material. T2 - RubberCon 2023 CY - Edinburgh, Scotland DA - 09.05.2023 KW - Hydrogen KW - Ageing KW - Seal PY - 2023 AN - OPUS4-58178 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Kömmling, Anja A1 - Simbruner, Kai A1 - Grelle, Tobias A1 - Jaunich, Matthias A1 - Zencker, Uwe A1 - Wolff, Dietmar A1 - Orellana Pérez, Teresa A1 - Völzke, Holger T1 - Research at BAM for evaluating long term safety of container systems and components N2 - Safety of long term containment and storage of radioactive waste is an essential issue, which is increasingly gaining international attention. Extending interim storage beyond initial license periods is one of the major challenges worldwide. BAM has been involved in all kinds of radioactive waste container safety evaluation for storage and transportation including their long term performance from the very beginning. Today, all work related to the safe management of radioactive waste is linked by the activity field “Nuclear Waste Management” within the Focus Area “Energy” at BAM and in conjunction with a research strategy and agenda. Most recently, the working group “Long Term Safety of Container Systems and Components” was established to launch and perform research projects related to safety issues concerning the extended interim storage of radioactive waste. For example, within our project LaMEP, we investigate ageing effects of metal and elastomer seals as well as polymeric neutron shielding materials, which are container components that fulfil major safety functions. The results of the experiments help to understand the long term behaviour of these components. Likewise, our project BRUZL started at BAM in 2018 with the aim of developing a fracture mechanics approach to understand and describe a potential brittle failure mechanism of fuel cladding during long-term interim storage. BAM also contributes to the GRS project “Development of methods and models and international exchange for safety evaluation in the frame of interim storage of radioactive waste”. Additionally, BAM is involved in several international research programmes dealing with extended interim storage, such as the European Joint Programme on Radioactive Waste Management (EURAD), the Extended Storage Collaboration Program (ESCP) and IAEA Coordinated Research Projects. The present contribution provides a comprehensive overview of BAM research activities contributing to national and international gap analyses and to filling knowledge gaps regarding the safe long term management of radioactive waste. T2 - Annual Meeting on Nuclear Technology 2019 CY - Berlin, Germany DA - 07.05.2019 KW - Radioactive Waste KW - Long-term safety PY - 2019 SN - 978-3-926956-95-8 SP - 1 EP - 5 AN - OPUS4-51486 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Kömmling, Anja A1 - Jaunich, Matthias A1 - Wolff, Dietmar T1 - Characterisation of degradation and determination of end-of-lifetime criterion for O-ring seals N2 - The ageing of polymers, including elastomers, is an undesirable but inevitable process leading to a limited lifetime of rubber products such as seals. Independent of the application, as e.g. in automotive, piping or container applications, a long lifetime or at least a timely exchange of a seal before occurrence of critical failure is desired. In order to investigate the degradation of material properties and to determine the lifetime of elastomers used as seals, an ageing programme was started with hydrogenated acrylonitrile butadiene rubber (HNBR), ethylene propylene diene rubber (EPDM) and fluorocarbon rubber (FKM) [1-3]. Both O-ring seals (uncompressed and compressed by 25 %) with a cord diameter of 10 mm as well as sheets with a thickness of 2 mm were aged at 75 °C, 100 °C, 125 °C and 150 °C for up to two years. The changes of material properties during ageing were characterised for each material using samples from the sheets by means of e.g. Dynamic Mechanical Analysis and tensile tests, while sealing properties such as leakage rate were determined on O-rings. The experimental results indicate that while material properties show considerable degradation effects, the static leakage rate stays constant or even decreases before failure occurs quite suddenly at advanced degradation levels. This reveals that static leakage rate has only limited sensitivity for the degradation of the seal material. Our approach to determine a suitable end of lifetime criterion, which involves a partial decompression of the seal during the leakage test, is presented and discussed. T2 - RubberCon 2017 CY - Prague, Czech Republic DA - 23.05.2017 KW - Life time prediction KW - Ageing KW - Rubber seal KW - Leakage PY - 2017 SN - 978-80-906662-0-7 SP - 65 EP - 72 AN - OPUS4-40391 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Grelle, Tobias A1 - Probst, Ulrich A1 - Wolff, Dietmar A1 - Jaunich, Matthias A1 - Völzke, Holger T1 - Investigations on the long-term behavior of metal seals for dual purpose casks N2 - In Germany, spent nuclear fuel and high active waste from reprocessing is stored in transport and storage containers with double lid systems that are equipped with metal seals completing the primary sealing barrier. The tasks of the Bundesanstalt für Materialforschung und -prüfung (BAM) within the interim storage licensing procedures ruled by the German Atomic Energy Act include the long-term safety evaluation of the container design regarding the permanently safe enclosure of the inventory. In order to generate a knowledge base for the safety evaluation, research regarding the long-term behavior of the critical components is performed. So far, the containers are licensed for an interim storage period of 40 years. However, due to significant delays in establishing a final repository, the required time span for interim storage is expected to increase significantly. Thus, a widespread investigation program is run to gain systematic data on the long-term behavior of the seals and to develop prediction models. Long-term seal investigations consider the development of their restoring seal force, their useable resilience and their achievable leakage rate caused by aging at temperatures ranging from room temperature up to 150 °C. This year, the total time span of the tests reaches 10 years. Furthermore, seal segments are aged at the selected temperatures for up to 300 days. From these segments additional information on the sealing behavior, changes of the seal contact and the material behavior is gained. This contribution deals with the current results of the long-term seal investigations at BAM. Furthermore, insights of the more in-depth component and material investigations of the metal seals with focus on the seal contact development are discussed and the ongoing work aiming for an analytical description of the thermo-mechanical aging effects on metal seals are presented. T2 - 19th International Symposium on the Packaging and Transportation of Radioactive Materials PATRAM 2019 CY - New Orleans, LA, USA DA - 04.08.2019 KW - Metal seal KW - Radioactive waste containers KW - Creep KW - Long-term behaviour PY - 2019 SP - 1 EP - 6 AN - OPUS4-49019 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Jaunich, Matthias A1 - Stark, Wolfgang T1 - Monitoring the vulcanization of rubber with ultrasound: Influence of material thickness and temperature N2 - In consideration of the influence of the curing reaction on the material properties of elastomers, it is very important to control the vulcanization process properly. As shown previously [1], the effects of the vulcanization reaction of an elastomer can be monitored by use of ultrasonic sound waves. This technique has to a certain degree a high similarity to the standard curemeter test according to ISO 6502 but can be applied also inside a production tool. So far, the method was only applied to the vulcanization of one compound at a given temperature and sample thickness. This is now complemented with measurements on another compound system at different temperatures and sample thicknesses. The expected effects of temperature and thickness on the curing behaviour were found by use of the ultrasound online control. KW - Vulcanization KW - Cure process KW - Ultrasound KW - Curemeter KW - Elastomer KW - Natural rubber PY - 2009 DO - https://doi.org/10.1016/j.polymertesting.2009.08.006 SN - 0142-9418 VL - 28 IS - 8 SP - 901 EP - 906 PB - Elsevier Science CY - Amsterdam [u.a.] AN - OPUS4-19959 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Buchholz, Uwe A1 - Jaunich, Matthias A1 - Stark, Wolfgang A1 - Habel, Wolfgang A1 - Petersson, B.A.T. T1 - Acoustic data of cross linked polyethylene (XLPE) and cured liquid silicone rubber (LSR) by means of ultrasonic and low frequency DMTA N2 - Partial discharges may cause damage to electrical insulation of high voltage equipment. They initiate elastic waves in the insulating material, e.g. in the stress cone of an outdoor termination. Localisation of the origin of such elastic waves can help to predict serious damaging processes in the electrical insulation. In order to measure and evaluate the wave propagation effects in typical multilayered elastomeric structures, knowledge of the material properties is required. The propagating velocity and the attenuation of longitudinal waves are important parameters. Values for these quantities found in the literature were not appropriate. Therefore, for cross-linked polyethylene (XLPE) and cured liquid silicone rubber (LSR), the longitudinal wave velocity and the attenuation were evaluated in the temperature interval from -20°C to 50°C and in the frequency range from 200 kHz to 600 kHz using a two-sample ultrasound technique. The loss factor was determined from these measured quantities. Additionally, low frequency Dynamic Mechanical Thermal Analysis (DMTA) was applied to investigate LSR and XLPE in a temperature interval between -100 and 50°C and to check qualitatively the ultrasound data. KW - Acoustic propagation KW - Cross linked polyethylene insulation KW - Mechanical variables measurement KW - Silicone rubber PY - 2012 DO - https://doi.org/10.1109/TDEI.2012.6180250 SN - 1070-9878 SN - 0018-9367 SN - 1558-4135 VL - 19 IS - 2 SP - 558 EP - 566 PB - Institute of Electrical and Electronics Engineers CY - New York, NY AN - OPUS4-26106 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CHAP A1 - Kömmling, Anja A1 - Wolff, Dietmar A1 - Jaunich, Matthias ED - van Breugel, K. ED - Koleva, D. ED - Beek, T. T1 - Investigation of long-term behaviour of elastomeric seals for transport and storage packages N2 - Elastomers are widely used as the main sealing materials in Containers for low- and intermediate-level radioactive waste and as an additional component fo metal seals in spent-fuel and high-level waste containers. According to appropriate guidelines and regulations, safe enclosure of the radioactive container contents has to be guaranteed for lengthy storage periods of at least 40 years. Therefore, the understanding of seal ageing behaviour is of high importance and has to be considered with regard to possible dynamic events taking place during transport after storage. An accelerated ageing approach for compressed seals is presented, as well as some first results. KW - O Ring KW - Ageing KW - Rubber seal PY - 2018 SN - 978-3-319-70192-9 DO - https://doi.org/10.1007/978-3-319-70194-3_2 SP - 17 EP - 25 PB - Springer AN - OPUS4-43248 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - Langzeituntersuchungen an Behälterwerkstoffen und -komponenten T2 - 4. RAM-Behältersicherheitstage CY - Berlin, Germany DA - 2014-03-26 PY - 2014 AN - OPUS4-30673 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias T1 - Investigations at BAM on Fuel Cladding Integrity and DPC Seal Performance N2 - The presentation provides an update on preliminary results from research projects in the area of long term performance of metal seals and fuel rod integrity as safety relevant components of spent fuel transport and storage casks for spent nuclear fuel. T2 - Extended Storage Collaboration Program (ESCP) winter meeting 2022 CY - Charlotte, NC, USA DA - 07.11.2022 KW - Metal seal KW - Fuel cladding KW - Ring compression test KW - Brittle failure PY - 2022 AN - OPUS4-56400 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - JOUR A1 - Jaunich, Matthias T1 - Editorial N2 - Dear Readers, a new year started for all of us (as I write these lines, possibly it was already some time ago when these lines are finally available) and this is the time for the so-called New Year’s resolutions. Setting goals and changing our behavior as well in a private as in a professional context. For Scientists the resolutions may comprise tasks like finalizing a longago started publication, picking up the loose ends of an application for funding or just bringing the running projects in a greater structure. KW - Editorial KW - Polymer Testing PY - 2019 DO - https://doi.org/10.1016/j.polymertesting.2019.01.010 SN - 0142-9418 VL - 74 SP - A1 PB - Elsevier AN - OPUS4-47406 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - GEN A1 - Jaunich, Matthias A1 - Stark, Wolfgang A1 - Wolff, Dietmar T1 - Messung des Tieftemperaturverhaltens von Elastomer-Dichtungen T2 - TECHNOMER 2009 - 21. Fachtagung über Verarbeitung und Anwendung von Polymeren CY - Chemnitz, Deutschland DA - 2009-11-12 KW - Dichtungen KW - Elastomere KW - Tieftemperaturverhalten PY - 2009 SN - 978-3-939382-09-6 IS - ETV7 SP - 1 EP - 9 AN - OPUS4-20386 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER -