TY - CONF A1 - Weber, Mike A1 - Zaghdoudi, Maha A1 - Kömmling, Anja A1 - Jaunich, Matthias A1 - Wolff, Dietmar T1 - A numerical approach to correlate compression stress relaxation and compression set of elastomer O-rings with tightness T2 - Proceedings of the ASME 2021 Pressure Vessels & Piping Conference (PVP2021) N2 - The excellent mechanical properties of elastomer seals at a wide range of temperatures as well as their high versatility and recovery potential under several load conditions make these materials well suitable for the application in containers designed for transport and disposal of negligible heat generating radioactive waste. While a seal exchange at defined intervals is typical in many conventional applications, it is impossible or at least hard to perform when principles of minimization of radiation exposure have to be considered which prohibit an avoidable cask handling. An extensive knowledge of the change of the elastomer properties during aging and the availability of reliable end-of-lifetime criteria to guarantee the safe enclosure of the radioactive material for the required time are mandatory. As BAM is involved in most of the national cask licensing procedures and in the evaluation of cask-related long-term safety issues, great efforts have already been made and are still ongoing to scientifically support this task. Among other representative types of elastomers, specimen made from ethylene propylene diene rubber (EPDM) were tested before, during and after aging to capture the with respect to application most important of their complex mechanical properties. Exemplary results of these investigations were used to calibrate material models implemented in the commercial finite element software ABAQUS/Standard®. The finite element model already presented in previous works uses a sequential temperature displacement coupling. The calculated compression stress relaxation (CSR) and compression set (CS) values do satisfactorily match the experimental results. In many investigations performed at BAM both values (CSR and CS) were identified as key indicators of elastomer’s long-term performance. However, the possibility to correlate these equivalent indicators with performance values such as tightness and leakage rate, measurable in the mounted state, is an important goal of our future work. In the presented study the ABAQUS® feature of “pressure penetration” is introduced in the suggested finite element model for this purpose. It provides the possibility to simulate the penetration of a gas into a possible gap between flange and O-ring causing an opening of a leakage path. Three dimensional and axis-symmetric finite element models were generated to represent flat and grooved flanges of different dimensions. The sensitivity of the feature to several input parameters is investigated and the observed behavior of the O-ring is correlated with the results of performed leakage tests. T2 - ASME 2021 Pressure Vessels & Piping Conference (PVP2021) CY - Online meeting DA - 13.07.2021 KW - Elastomer KW - Tightness KW - Leakage KW - Compression set KW - Compression stress relaxation PY - 2021 SN - 978-0-7918-8535-2 DO - https://doi.org/10.1115/PVP2021-61976 SP - 1 EP - 8 PB - American Society of Mechanical Engineers (ASME) CY - New York, NY, USA AN - OPUS4-54422 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Kömmling, Anja A1 - Jaunich, Matthias A1 - Wolff, Dietmar T1 - Ageing and lifetime prediction of O-ring seals made of HNBR, EPDM and FKM T2 - 12. Kautschuk Herbst Kolloquium N2 - BAM is the federal institute for materials research and testing in Germany. One of our tasks is to evaluate the safety of casks designed for transport and/or storage of radioactive waste. As elastomeric seals are used in the containers as safety-relevant parts, it is our goal to be able to evaluate the service lifetime of the seals with regard to the requirements for long-term safety (40 years and more) of the containers. For this reason, an accelerated ageing programme with selected rubbers often used for seals (HNBR, EPDM and FKM) was started. Ageing was performed at four different temperatures (75 °C, 100 °C, 125 °C and 150 °C) for up to 2 years. For assessing properties related to the sealability, O-rings were aged in compression by 25 % (corresponding to the compression during service) between plates. For comparison, uncompressed O-rings were aged as well. The aged materials were characterized with conventional polymer analysis methods such as hardness and tensile tests, but also with more seal-specific methods such as compression stress relaxation (CSR, reflecting the loss of sealing force of a compressed seal over time), and compression set (CS, representing the recovery behaviour of a seal after release from compression). CS is chosen as the property for lifetime prediction as it is both sensitive to degradation and related to the seal performance. CS data is extrapolated to 60 °C, which yields lifetimes of approximately 5 years for HNBR and 64 years for EPDM for a criterion of 85 % CS respectively, and approx. 40 years for FKM for a criterion of 65 % CS (the highest value measured so far). T2 - 12. Kautschuk Herbst Kolloquium CY - Hanover, Germany DA - 22.11.2016 KW - Rubber KW - Compression set KW - Extrapolation KW - Degradation PY - 2016 SN - 9783981407648 VL - 2016 AN - OPUS4-38483 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Kömmling, Anja A1 - Jaunich, Matthias A1 - Wolff, Dietmar T1 - Ageing of elastomeric seals for storage containers T2 - Annual Meeting on Nuclear Technology 2015 N2 - At BAM Federal Institute for Materials Research and Testing in Germany, it is our responsibility to audit the safety of casks designed for transport and/or storage of radioactive material. With regard to the requirements on long-term safety of the containers, it is necessary to evaluate the service lifetime of the elastomeric seals used in the containers. With ageing, the elastomers will gradually lose their elasticity and their ability for recovery, which might result in a leakage above the allowed level or in a release of radioactivity during an incident. It is important to know the rate of degradation and which property can be used as an practical and easily measurable end-of-lifetime criterion. For this reason, we devised ageing experiments on different kinds of elastomers, namely FKM, EPDM and HNBR. The former two are actually used in containers for radioactive wastes – either as auxiliary seal in casks containing high activity waste, or as main seal in casks for medium or low activity waste. The latter is an often used seal material that is tested for comparative reasons. In our ageing program, these three materials are aged at four different temperatures (75 °C, 100 °C, 125 °C and 150 °C) in order to extrapolate the data to service temperature using a suitable model. They are examined at logarithmic time intervals of several days up to 5 years. The samples are aged in their undeformed O-ring state as well as compressed between flanges with a deformation corresponding to the actual compression during service. Thus we can compare the ageing between relaxed and stressed sample. Additionally, we are ageing samples in flanges that allow leakage rate measurements. Other measurements include monitoring of the recovery force of the seal and the compression set. Furthermore, the samples are examined by thermal and dynamic-mechanical analysis for detecting changes in the glass transition temperature due to crosslinking or chain scission in the material. Besides, hardness is measured as a practical macroscopic indicator. Until now, we have analyzed samples aged up to 100 days. At the highest ageing temperature of 150 °C, the compressed EPDM has already reached a compression set of 95 %, while HNBR and FKM have reached 80 % and 30 %, respectively. Furthermore, HNBR has reached a Shore D hardness of 85, which is an immense increase after the initial value of 80 Shore A. However, when looking at the cross-section of the sample, it was obvious that only a layer of about 1 mm thickness has become so hard, while the inner part remained rubbery. This shows that there has been intense crosslinking mostly near the surface of the HNBR which forms a kind of oxygen diffusion barrier, inhibiting the thermooxidation of the inner part of sample which can retain elastic properties. In EPDM, the oxygen permeability is much greater, which leads to a more homogeneous degradation across the whole sample and thus resulted in a higher compression set. The low compression set of FKM shows the outstanding high-temperature properties of this material. T2 - Annual Meeting on Nuclear Technology 2015 CY - Berlin, Germany DA - 2015-05-05 KW - Elastomer KW - Rubber KW - Aging KW - Lifetime KW - Seal KW - Cask KW - Compression PY - 2015 SN - 978-3-926956-98-9 SP - 1 EP - 10(?) PB - INFORUM-Verl. u. Verwaltungsges. AN - OPUS4-33782 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Kömmling, Anja A1 - Jaunich, Matthias A1 - Wolff, Dietmar T1 - Ageing of elastomeric seals for storage containers T2 - IRC 2015 - International rubber conference / DKT 2015 - Deutsche Kautschuk-Tagung N2 - At BAM Federal Institute for Materials Research and Testing in Germany, it is our responsibility to evaluate the safety of casks designed for transport and/or storage of radioactive material. This includes the investigation of elastomeric seals applied in the containers. Besides examining the low-temperature behavior of elastomeric seals, it is our goal to evaluate the service lifetime of the seals with regard to the requirements for long-term safety (40 years and more) of the containers. Furthermore, we deem it necessary to exceed the requirements given in the ageing standard DIN 53508 and take into account diffusion-limited oxidation (DLO) effects and non-Arrhenius behavior when making lifetime predictions. Therefore, we started an ageing programme with selected rubbers (HNBR, FKM and EPDM) which are oven-aged at four different temperatures (75 °C, 100 °C, 125 °C and 150 °C) in order to extrapolate the data to service temperature using different models and check which one is appropriate. Samples are examined at different times up to 5 years. In order to be able to compare between compressed and relaxed rubber, they are aged in two conditions: the undeformed O-ring state as well as compressed between plates with a compression of 25 % corresponding to the actual compression during service. Additionally, we are ageing samples in flanges that allow leakage rate measurements which is the central performance criterion. Analysis methods include hardness as a quick indicator, compression set and compression stress relaxation as measures reflecting the actual properties of a compressed seal. Additionally, we are applying classical polymer analysis methods like dynamic mechanic analysis and thermogravimetric analysis which show changes in the polymeric structure due to chain scission and crosslinking. Furthermore, we are testing the leakage rate of the O-rings in order to correlate the changes in physical properties to the actual performance of the seal. First results of samples aged up to 100 days show a strong increase in hardness for HNBR, a moderate increase for EPDM and hardly a change for FKM. A similar result is seen in the compression set of samples aged 100 d at 100 °C in compression as HNBR has reached 60 %, EPDM 25 % and FKM 15 % compression set. However, after ageing at 150 °C, EPDM shows a worse performance with 95 % compression set compared to HNBR with only 80 %. This is probably due to DLO effects in HNBR that appear because of the fast ageing and low oxygen permeability in HNBR. This leads to a deficit of oxygen in the center of the sample which is thus protected from ageing and can retain elastic properties. The full paper shall discuss the changes in material properties observed to date and the impact on the performance of elastomeric seals. T2 - IRC 2015 - International rubber conference CY - Nürnberg, Germany DA - 29.06.2015 KW - Elastomer KW - Rubber KW - Aging KW - Lifetime KW - Seal KW - Cask KW - Compression PY - 2015 SP - 1 EP - 10 AN - OPUS4-34939 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Kömmling, Anja A1 - Jaunich, Matthias A1 - Wolff, Dietmar T1 - Aging of elastomeric seals for storage casks T2 - WM2015 Conference (Proceedings) N2 - Elastomeric seals are used in many containers, including casks for radioactive waste. However, like all polymers, elastomers are prone to aging, which leads to a loss of sealing force and the ability for recovery which can ultimately result in leakage. Therefore it is important to be able to define an end-of-lifetime criterion and to judge the lifetime of elastomeric seals. For this reason, we started an aging program on three kinds of rubbers (HNBR, EPDM, FKM), monitoring the change of properties at four different aging temperatures over extended periods up to five years. The measured data is used for lifetime prediction by applying a suitable model. T2 - WM2015 Conference CY - Phoenix, Arizona, USA DA - 15.03.2015 KW - Aging KW - Elastomer KW - Seal KW - Leakage KW - Compression PY - 2015 SN - 978-0-9828171-4-8 SP - 15080, 1 EP - 12 AN - OPUS4-33253 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Subramani Bhagavatheswaran, E. A1 - Wießner, S. A1 - Jaunich, Matthias A1 - Wolff, Dietmar T1 - Aging study and electrical resistance based stress-monitoring of rubber seals T2 - 192nd Technical meeting of the ACS Rubber Division N2 - Elastomer seals are widely used as barrier seals in containers for low and intermediate level radioactive waste. In addition, they are also used in waste fuel storage and transportation casks as auxiliary seals. Depending on the area of use, the rubber materials have to demonstrate proper sealing performance with respect to mechanical, thermal and environmental conditions as well as irradiation during the entire operation period. A fundamental understanding of the structure property relationship and their changes during aging can help to evaluate the long-term sealing performance. In the present study, specific materials are investigated to study the structure-property and seal performance-correlation. Fluoro-elastomer (FKM), silicone rubber (VMQ) and ethylene propylene diene rubber (EPDM) were chosen as base rubbers. Comparable mechanical properties for these seals, especially in terms of a comparable compression behavior were achieved by careful control of base rubber formulation, i.e., by opting for the right filler and its concentration, amount of crosslinking chemicals, and with the assistance of process oils. Moreover, with the same rubber, similar mechanical properties were achieved by varying the filler concentration and crosslinking degree, which shall enable to correlate the particular influence on the structure property dependency of the seals in detail. The materials are investigated under pristine and aged conditions to evaluate the influence of aging, e.g. on the stress relaxation or recovery behavior. These values appear to be suitable parameters to judge the expected sealing performance. Due to the electrically conducting nature of some fillers used to reinforce rubbers (such as carbon blacks, carbon nanotubes (CNTs), Graphene, etc.) it is possible to obtain current information about mechanical and visco-elastic properties by monitoring the electrical conductivity or resistivity. A simple relation that relates electrical resistance with mechanical stress was derived and the stress values were theoretically predicted from the electrical resistance values, which showed good correlation with experimental results. T2 - 192nd Technical meeting of the ACS Rubber Division CY - Cleveland, OH, USA DA - 09.10.2017 KW - Seal KW - Rubber KW - Degradation KW - Structure-property relationship KW - Ageing PY - 2017 VL - 2017 SP - 1 EP - 25 AN - OPUS4-42849 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Kömmling, Anja A1 - Jaunich, Matthias A1 - Wolff, Dietmar T1 - Alterung von Elastomerdichtungen für Lagerbehälter T2 - Technomer 2015 - 24. Fachtagung über Verarbeitung und Anwendung von Polymeren N2 - Unsere Aufgabe im Fachbereich 3.4 der Bundesanstalt für Materialforschung und prüfung (BAM) ist die sicherheitstechnische Begutachtung von Transport- und Lagerbehältern für radioaktiven Abfall, die für langfristige Zwischenlagerung ausgelegt sind. Ein Arbeitsschwerpunkt ist die Bewertung der Lebensdauer von Metall- und Elastomerdichtungen in den Behältern im Hinblick auf die Anforderungen für langfristige Behältersicherheit (min. 40 Jahre in Deutschland). Um die Eigenschaftsänderungen der Elastomerdichtungen während einer beschleunigten Alterung über lange Zeiträume (bis zu fünf Jahre) untersuchen zu können, wurde ein Alterungsprogramm an ausgewählten Elastomeren (HNBR, EPDM, FKM) begonnen. Im Gegensatz zu Normalterungsverfahren altern wir keine Normteile, sondern O-Ringe im unverpressten sowie verpressten Zustand. Diese Vorgehensweise ermöglicht die Bewertung des Einflusses der Verpressung auf die Alterung sowie die Untersuchung des Bauteilversagens mittels Leckageratenmessungen unter anwendungsnahen Bedingungen. Weitere Charakterisierungsmethoden sind Härtemessung, dynamisch-mechanische Analyse (DMA), Thermogravimetrie (TGA), Druckspannungsrelaxation, Druckverformungsrest (DVR), Dichtebestimmung und Zugversuch. Das Ziel ist, die Leckagerate mit anderen Eigenschaften bzw. Methoden zu korrelieren, um so ein aussagekräftiges und leichter zu bestimmendes Lebensdauerkriterium für elastomere O-Ringe abzuleiten. Während der Alterung können in Abhängigkeit von Material sowie Alterungsdauer und –temperatur Inhomogenitäten aufgrund von diffusionsbegrenzter Oxidation auftreten, durch die sich unterschiedliche Eigenschaften an der Oberfläche und im Volumen der Dichtung ergeben, was zu falschen Lebensdauerabschätzungen führen kann. Mittels Mikrohärtemessung über den Querschnitt werden diese Effekte charakterisiert und bei der Extrapolation mittels Zeit-Temperatur-Verschiebung und Arrheniusgraph berücksichtigt. Bisher liegen Daten von bis zu einem Jahr bei vier verschiedenen Temperaturen (75 °C, 100 °C, 125 °C und 150 °C) gealterten Proben vor. Nach 100 Tagen bei 150 °C weisen HNBR und EPDM schon einen DVR von über 80 % auf, aber noch keinen signifikanten Anstieg der Leckagerate. Diese sinkt zunächst während der Alterung, da die Permeabilität aufgrund von Vernetzungsreaktionen sinkt. Bei HNBR ist dies aufgrund der dominanteren Vernetzungsreaktionen während der Alterung noch stärker ausgeprägt als bei EPDM. T2 - Technomer 2015 - 24. Fachtagung über Verarbeitung und Anwendung von Polymeren CY - Chemnitz, Germany DA - 12.11.2015 KW - Aging KW - Elastomer KW - Seal KW - Leakage KW - Compression PY - 2015 SN - 978-3-939382-12-6 SP - 43 CY - Chemnitz AN - OPUS4-35050 LA - deu AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias A1 - Wolff, Dietmar T1 - An approach to improve the understanding of elastomeric seals in use in storage containers T2 - 45th Annual meeting on nuclear technology (Proceedings) N2 - Elastomers are widely used as main sealing materials in Containers for low and intermediate level radioactive waste and as additional component to metal seals in spent fuel and high active waste Containers. They are applied due to their special material properties and easy use [1]. For this application several challenging prerequisites must be met for the essential reliable Operation of the seal. T2 - 45th Annual meeting on nuclear technology CY - Frankfurt, Germany DA - 06.05.2014 PY - 2014 SN - 978-3-926956-99-6 SP - 1 EP - 4 AN - OPUS4-31250 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Agroui, K. A1 - Jaunich, Matthias A1 - Hadj Arab, A. T1 - Analysis techniques of polymeric encapsulant materials for photovoltaic modules: Situation and perspectives T2 - Africa-EU Symposium on renewable energy research and innovation N2 - The properties of the encapsulant are critical to the long-term performance of photovoltaic (PV) modules under the influence of sunlight including UV, elevated temperature, humidity and diffusion of oxygen. Encapsulation process represents about 40% of the whole PV module cost. The introduction of new non-EVA encapsulant material type “Low-Cost, High-Performance” should provide a solution to outdoor yellowing degradation problems. The emerging encapsulant materials exhibit a good compatibility with emerging PV solar cells for long term durability. This new generation of encapsulant materials has the advantage to improve the PV module performances and long term durability for specific climate like desert regions. This scientific contribution presents an overview of the different encapsulant materials currently on the market, the general requirements of the emerging encapsulant materials and characterizations techniques for degradation, diagnostic and reliability lifetime estimation in the framework of Algerian renewable energy strategy. T2 - Africa-EU Symposium on Renewable Energy Research and Innovation CY - Tlemcen, Algeria DA - 08.03.2016 KW - solar cells KW - PV modules KW - polymer encapsulant KW - encapsulation KW - analysis techniques PY - 2016 SP - 27 EP - 27 PB - European Union Energy Initiative – Partnership Dialogue Facility (EUEI PDF) CY - Eschborn, Germany AN - OPUS4-35917 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Jaunich, Matthias A1 - Wolff, Dietmar ED - Van Breugel, K. ED - Koenders, E.A.B. T1 - Approach for the investigation of long-term behaviour of elastomeric seals for transport and storage packages T2 - AMS 14 - Ageing of materials & structures - Proceedings of the 1st ageing of materials & structures 2014 conference N2 - Elastomers are widely used as main sealing materials for Containers for low and intermediate Ievel radioactive waste and as additional component to metal seals in spent fuel and high active waste Containers. According to appropriate guidelines and regulations safe enclosure of the radioactive Container contents has to be guaranteed for long storage periods as well as down to temperatures of -40 °C for transportation. Therefore the understanding of seal behaviour in general is of high importance and ageing of elastomeric seals has to be considered with regard to possible dynamic events taking possibly place during transport after storage. T2 - 1st Ageing of materials & structures 2014 conference CY - Delft, The Netherlands DA - 26.05.2014 KW - O-Ring KW - Seal KW - Ageing KW - Elastomer KW - Compression set PY - 2014 SN - 978-94-6186-313-3 SP - 87 EP - 93 AN - OPUS4-30820 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER -