TY - JOUR A1 - Kirner, Sabrina V. A1 - Slachciak, Nadine A1 - Elert, Anna M. A1 - Griepentrog, Michael A1 - Fischer, Daniel A1 - Hertwig, Andreas A1 - Sahre, Mario A1 - Dörfel, Ilona A1 - Sturm, Heinz A1 - Pentzien, Simone A1 - Koter, Robert A1 - Spaltmann, Dirk A1 - Krüger, Jörg A1 - Bonse, Jörn T1 - Tribological performance of titanium samples oxidized by fs-laser radiation, thermal heating, or electrochemical anodization N2 - Commercial grade-1 titanium samples (Ti, 99.6%) were treated using three alternative methods, (i) femtosecond laser processing, (ii) thermal heat treatment, and (iii) electrochemical anodization, respectively, resulting in the formation of differently conditioned superficial titanium oxide layers. The laser processing (i) was carried out by a Ti:sapphire laser (pulse duration 30 fs, central wavelength 790 nm, pulse repetition rate 1 kHz) in a regime of generating laser-induced periodic surface structures (LIPSS). The experimental conditions (laser fluence, spatial spot overlap) were optimized in a sample-scanning setup for the processing of several square-millimeters large surface areas covered homogeneously by these nanostructures. The differently oxidized titanium surfaces were characterized by optical microscopy, micro Raman spectroscopy, variable angle spectroscopic ellipsometry, and instrumented indentation testing. The tribological performance was characterized in the regime of mixed friction by reciprocating sliding tests against a sphere of hardened steel in fully formulated engine oil as lubricant. The specific tribological performance of the differently treated surfaces is discussed with respect to possible physical and chemical mechanisms. KW - Femtosecond laser KW - Titanium KW - Oxidation KW - Friction PY - 2018 U6 - http://nbn-resolving.de/urn/resolver.pl?urn:nbn:de:kobv:b43-445609 UR - http://gateway.webofknowledge.com/gateway/Gateway.cgi?GWVersion=2&SrcAuth=Alerting&SrcApp=Alerting&DestApp=WOS&DestLinkType=FullRecord;UT=WOS:000428454200045 SN - 0947-8396 SN - 1432-0630 VL - 124 IS - 4 SP - 326, 1 EP - 10 PB - Springer-Verlag AN - OPUS4-44560 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bonse, Jörn A1 - Kirner, Sabrina A1 - Slachciak, Nadine A1 - Elert, Anna A1 - Griepentrog, Michael A1 - Hertwig, Andreas A1 - Sahre, Mario A1 - Weise, Matthias A1 - Sturm, Heinz A1 - Pentzien, Simone A1 - Koter, Robert A1 - Spaltmann, Dirk A1 - Krüger, Jörg T1 - Tribological performance of titanium samples oxidized by fs-laser radiation, thermal heating, or electrochemical anodization N2 - Commercial grade-1 titanium samples (Ti, 99.5% purity) were treated using three alternative methods, i.e., fs-laser processing in air, thermal heat treatment in an oven, or anodization in an electrochemical bath, all resulting in the formation of differently conditioned superficial oxide layers. The laser processing was carried out by a Ti:sapphire laser (pulse duration 30 fs, central wavelength 790 nm, pulse repetition rate 1 kHz) in a regime of generating laser-induced periodic surface structures (LIPSS). The experimental conditions (laser fluence, spatial spot overlap) were optimized in a sample-scanning geometry for the processing of several square-millimetres large surface areas covered homogeneously by these nanostructures. The thermal processing in the oven was done at two different temperatures, while the electrochemical anodization was performed at room temperature, aiming to generate different polymorphs of titanium oxide at similar oxide layer thickness. The irradiated surface regions were characterized by optical and scanning electron microscopy, and micro Raman spectroscopy. The tribological performance of the differently treated titanium surfaces was characterized in the regime of mixed friction by reciprocating sliding tests against a sphere of hardened steel in un-additivated paraffin oil and fully formulated engine oil as lubricants. The specific tribological performance of the differently treated surfaces is discussed on the basis of possible physical and chemical mechanisms. T2 - International Conference on Laser Ablation, COLA 2017 CY - Marseille, France DA - 03.09.2017 KW - Femtosecond laser KW - Oxidation KW - Laser-induced periodic surface strcutures, LIPSS KW - Friction KW - Wear PY - 2017 AN - OPUS4-42032 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bonse, Jörn A1 - Kirner, Sabrina V. A1 - Wirth, Thomas A1 - Spaltmann, Dirk A1 - Krüger, Jörg T1 - Chemical effects in the formation of fs-laser-induced periodic surface structures N2 - The processing of laser-induced periodic surface structures (LIPSS, ripples) on metals and semiconductors in ambient air is usually accompanied by superficial oxidation effects - widely neglected in the current literature. In this contribution, chemical, structural, and mechanical alterations in the formation of femtosecond LIPSS are characterized by a variety of surface analytical techniques, including energy dispersive X-ray analyses (EDX), X-ray photoelectron spectroscopy (XPS), micro Raman spectroscopy (µ-RS), and depth-profiling Auger electron microscopy (AEM). Alternative routes of electrochemical and thermal oxidation allow to qualify the relevance of superficial oxidation effects on the tribological performance in oil lubricated reciprocating sliding tribological tests (RSTT). It is revealed that the fs-laser processing of near-wavelength sized LIPSS on metals leads to the formation of a few hundreds of nanometer thick graded oxide layer, consisting mainly of amorphous oxides. Regardless of its reduced hardness and limited thickness, this nanostructured surface layer can effciently prevent a direct metal-metal contact in the RSTT and may also act as an anchor layer for specific wear-reducing additives contained in the engine oil involved T2 - 8th International LIPSS Workshop CY - Bochum, Germany DA - 27.09.2018 KW - Laser-induced periodic surface structures, LIPSS KW - Femtosecond KW - Oxidation KW - Tribology PY - 2018 AN - OPUS4-46106 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER - TY - CONF A1 - Bonse, Jörn A1 - Kirner, Sabrina V. A1 - Wirth, Thomas A1 - Florian, Camilo A1 - Sturm, Heinz A1 - Spaltmann, Dirk A1 - Krüger, Jörg T1 - Chemical effects during the formation of femtosecond laser-induced periodic surface structures N2 - The processing of laser-induced periodic surface structures (LIPSS, ripples) on metals and semiconductors in ambient air is usually accompanied by superficial oxidation effects – a fact that is widely neglected in the current literature. In this contribution, chemical, structural, and mechanical alterations in the formation of femtosecond LIPSS are characterized by a variety of surface analytical techniques, including energy dispersive X-ray analyses (EDX), X-ray photoelectron spectroscopy (XPS), micro Raman spectroscopy (µ-RS), and depth-profiling Auger electron microscopy (AEM). Alternative routes of electrochemical and thermal oxidation allow to qualify the relevance of superficial oxidation effects on the tribological performance in oil lubricated reciprocating sliding tribological tests (RSTT). It is revealed that the fs-laser processing of near-wavelength sized LIPSS on metals leads to the formation of a few hundreds of nanometers thick graded oxide layers, consisting mainly of amorphous oxides. Regardless of reduced hardness and limited thickness, this nanostructured surface layer efficiently prevents a direct metal-to-metal contact in the RSTT and may also act as an anchor layer for specific wear-reducing additives contained in the used engine oil. T2 - EMRS Spring Meeting 2019, Symposium V “Laser interactions with materials: from fundamentals to applications" CY - Nice, France DA - 27.05.2019 KW - Laser-induced periodic surface structures (LIPSS) KW - Femtosecond laser KW - Oxidation KW - Tribology PY - 2019 AN - OPUS4-48127 LA - eng AD - Bundesanstalt fuer Materialforschung und -pruefung (BAM), Berlin, Germany ER -